GB/T 714 Q420qD bridge steel plate stacked at SHH STEEL warehouse

GB/T 714 Q420qD Bridge Steel Plate Supplier

GB/T 714 Q420qD is bridge structural steel plate with 420 MPa minimum yield, 540 MPa minimum tensile and Charpy V-notch impact of 120 J at −20°C for 12–100 mm plate. SHH STEEL supplies Q420qD mill-direct, TMCP / TMCP+T, up to 130 mm, with Z15–Z35, UT and heat and product analysis.
Keywords
Q420qD, Q420qD steel plate, GB/T 714 Q420qD, Q420q-D, Q420q D, Q420qD bridge steel, Q420qDZ15, Q420qDZ25, Q420qDZ35, bridge steel plate, Q420qD supplier
Equivalent Grades:
EN 10025-4 S420M, S420ML (Annex B) / ASTM A572 Gr.60 (strength only) — Material Specification: GB/T 714-2025 (supersedes GB/T 714-2015) — Delivery: TMCP / TMCP+T
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q420q Quality Grades
GB/T 714-2025 vs 2015
Q420qD vs ASTM A709 / EN 10025
TMCP vs Normalized vs QT
Welding and Fatigue
Z15 / Z25 / Z35
Equivalent Material Grades
Testing and Inspection
Dimensions
Tolerances
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 714 Q420qD Bridge Steel Plate?

Q420qD is bridge structural steel plate to GB/T 714. Q stands for yield, 420 is the minimum yield in MPa for plate up to 50 mm, q stands for qiao (bridge) and D is the quality grade: Charpy V-notch at −20°C on longitudinal specimens.

Q420q is the first of the lean-carbon high-strength bridge grades (C ≤0.11%), used for main trusses and box girders on long-span bridges. Q420q moves to a C ≤0.11% TMCP chemistry and is judged by Pcm (≤0.22%) instead of CEV. China’s first large Q420qE application was the Nanjing Dashengguan Yangtze River Bridge, a six-track high-speed railway arch bridge.

Q420qD is the entry point to the lean-carbon high-strength family: C ≤0.11%, Pcm ≤0.22%, 420 MPa yield and −20°C Charpy. It is common on cable-stayed box girders and long-span truss chords in temperate zones.

GB/T 714-2025 is the current edition. It was issued on 31 October 2025, took effect on 1 May 2026 and fully supersedes GB/T 714-2015, the fourth revision since the standard was first issued in 1965. We certify to the edition written on the purchase order.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q420qD cut to size with an EN 10204 3.1 or 3.2 certificate. Sister grades are listed under GB/T 714.

Material Specification

Specification element Requirement SHH STEEL compliance
Standard GB/T 714-2025 Q420qD Confirmed
Product Single-rolled plate ≤150 mm; hot-rolled strip and cut plate ≤25.4 mm Plate
Thickness with tensile values Up to 130 mm for Q420q Confirmed
Minimum yield ReL 420 MPa ≤50 mm; 410 MPa >50–100 mm Confirmed
Minimum tensile Rm 540 MPa ≤100 mm (no upper limit in the standard) Confirmed
Elongation A ≥ 19% Confirmed
Charpy V-notch −20°C, 120 J (12–100 mm), longitudinal Confirmed
Delivery condition TMCP or TMCP + tempering As ordered
Weldability index Pcm (Table 7) Printed on MTC
Ultrasonic testing Plate >20 mm: GB/T 2970, Class II or better Every plate
Through-thickness Z15, Z25 or Z35 to GB/T 5313, when ordered As ordered
Dimensions GB/T 709 Confirmed
Certificate GB/T 247; EN 10204 3.1 or 3.2 As ordered

Grades often compared with Q420qD are EN 10025-4 S420M, EN 10025-4 S420ML and ASTM A572 Gr.60; the comparison below shows where they differ.

Chemical Composition: Heat Analysis and Product Analysis

Third-party labs test plate, not ladles. So when an inspector checks Q420qD, the result is a product analysis and must be compared with product limits, not with the heat limits on the certificate.

Table 1 below is the heat (ladle) analysis for Q420qD from GB/T 714-2025 Tables 1, 3.

Element Q420qD TMCP (%)
C, max 0.11
Si, max 0.55
Mn 0.80 – 1.70
P, max 0.025
S, max 0.015
Nb 0.010 – 0.090
V 0.010 – 0.080
Ti 0.006 – 0.030
Als 0.010 – 0.045
Cr, max 0.50
Ni, max 0.30
Cu, max 0.30
Mo, max 0.20
N, max 0.0080
B, max 0.0005 residual (≤0.0014 if C ≤0.10%)
H, max 0.0002

Nb, V, Ti and Al may be added singly or together. Added singly, each must meet the range above; added together, at least one must reach its minimum and Nb + V + Ti ≤ 0.22%.

Table 2 is the product analysis: the limits a check analysis on finished plate is judged against. GB/T 714-2025 clause 7.1.3 calls up GB/T 222 for the permitted deviations.

Element Heat limit (%) Deviation, GB/T 222-2025 Table 1 Q420qD product analysis (%)
C ≤ 0.11 +0.02 ≤ 0.13
Si ≤ 0.55 +0.05 ≤ 0.60
Mn 0.80 – 1.70 ±0.06 0.74 – 1.76
P ≤ 0.025 +0.005 ≤ 0.030
S ≤ 0.015 +0.005 ≤ 0.020
V 0.010 – 0.080 +0.02 / −0.01 ≤ 0.100
Ti 0.006 – 0.030 +0.02 / −0.01 ≤ 0.050
Nb 0.010 – 0.090 ±0.005 (listed for 0.015–0.060%) Above 0.060%: agree in contract
Cr ≤ 0.50 +0.05 ≤ 0.55
Ni ≤ 0.30 +0.05 ≤ 0.35
Cu ≤ 0.30 +0.05 ≤ 0.35
Als 0.010 – 0.045 ±0.003 Lower limit −0.003 (Table 1 row is for Al ≥0.015%; confirm)
Mo ≤ 0.20 Not listed in Table 1 Agree in contract
N ≤ 0.0080 Listed only for 0.010–0.020% Agree in contract

How to read Table 2. Q420q TMCP heats are low-alloy steel, so Table 1 of GB/T 222 applies. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn falls in the 0.80–1.70% band, so ±0.06%. For one heat, an element may deviate in one direction only.

Mechanical Properties

Tensile values follow Table 9 of GB/T 714-2025 for Q420q. Tensile specimens are transverse; round specimens are used above 40 mm. Where yield is not distinct, Rp0.2 replaces ReL.

Nominal thickness ReL min (MPa) Rm min (MPa) A min
≤ 50 mm 420 540 19%
> 50 – 100 mm 410 540 19%
> 100 – 130 mm 365 460 19%

Impact values follow Table 10, on longitudinal specimens, average of three:

Letter / test temperature KV2 ≤12 mm KV2 >12 – 100 mm KV2 >100 – 150 mm
D / −20°C 80 J 120 J 47 J

One single value may fall below the required average, but not below 70% of it. Plate over 8 mm and under 12 mm is tested with 7.5 mm specimens (75% of the value); 6–8 mm plate with 5 mm specimens (50%). Plate under 6 mm is not impact tested.

180° bend test, transverse: mandrel D = 2a up to 16 mm and 3a above 16 mm; may be omitted when the mill guarantees it. Yield ratio is not mandatory. If the contract asks for it, Annex C recommends ReL/Rm ≤ 0.88 up to 12 mm and ≤ 0.86 above 12 mm for TMCP plate.

Q420qD / Q420qE / Q420qF: Which Quality Grade?

Q420qD is tested at −20°C. It suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C. D is the most specified letter on Chinese bridge drawings. It is tested at −20°C and the melt is tighter than C: P ≤0.025%, S ≤0.015%.

Grade Test temp. KV2 ≤12 mm KV2 12–100 mm KV2 >100 mm P / S max (%)
Q420qD −20°C 80 J 120 J 47 J 0.025 / 0.015
Q420qE −40°C 80 J 120 J 31 J 0.020 / 0.010
Q420qF −60°C By agreement 47 J — 0.015 / 0.006

Over-specifying the letter costs money; under-specifying it costs safety. Choose from the lowest service or erection temperature, then step up one letter for thick, restrained or fracture-critical members.

Q420qD: What Changed from GB/T 714-2015 to GB/T 714-2025

For Q420qD buyers the 2025 edition changes more than the year on the certificate. The points below come from the foreword of GB/T 714-2025 and its tables.

  • Yield values above 100 mm were added (365 MPa for >100–130 mm).
  • The Mn range for TMCP steel was revised: the minimum is now 0.80%, and the maximum may be raised to 2.00% by agreement.
  • CEV and Pcm limits were revised (Tables 6 and 7).
  • Tensile strength is now banded by thickness (e.g. lower minimum Rm above 100 mm) instead of one value.
  • Impact energy is set by thickness band (≤12 mm, 12–100 mm, >100 mm) in Table 10.
  • Yield ratio is no longer a clause value; it is agreed in the contract, with recommendations in informative Annex C.
  • Section products were removed; the standard now covers plate and strip only.
  • Delivery is TMCP, TMCP + tempering or QT; normalizing is kept only for Q345q/Q370q plate over 100 mm by agreement.

If a drawing cites 2015 and the plate is made to 2025, get the designer’s written acceptance; tensile strength above 100 mm and the yield-ratio basis differ.

Q420qD vs ASTM A709 and EN 10025: Which Grade Matches?

Can Q420qD replace a US or European bridge grade, or the other way round? Strength can match; toughness rules differ in kind, not only in number.

Property Q420qD EN 10025-4 S420M EN 10025-4 S420ML ASTM A572 Gr.60
Min. yield (MPa) 420 (≤50 mm) 420 (≤16 mm) 420 (≤16 mm) 415
Tensile (MPa) 540 min 520 – 680 520 – 680 520 min
Charpy 120 J at −20°C (12–100 mm) 40 J at −20°C 27 J at −50°C Supplementary only
Weathering chemistry No No No No

ASTM A709 sets Charpy requirements by temperature zone (1, 2, 3) and by member type: non-fracture-critical (T) or fracture-critical (F). GB/T 714 sets one value per letter, so compare the A709 zone with the GB/T 714 test temperature, not grade with grade.

EN 10025-3/-4/-6 grades show yield at the thinnest band; their values fall with thickness. GB/T 714 keeps 420 MPa to 50 mm. EN tensile ranges have upper limits; GB/T 714 gives minimums only.

The 120 J requirement in GB/T 714 for 12–100 mm plate is several times the 27–40 J typical of general structural grades. That margin is the main reason bridge owners specify Q420qD rather than GB/T 1591 plate.

Q420qD Delivery Condition: TMCP vs Normalized vs Quenched and Tempered

GB/T 714-2025 clause 3.2 defines TMCP as rolling with the final deformation in a controlled temperature range, including accelerated cooling with or without tempering (self-tempering included) but excluding direct quenching and quench-and-temper. The delivery route must be stated on the certificate.

Route Available for Q420qD Weldability index Notes
TMCP Yes, standard Pcm (C ≤0.11%) Up to 130 mm
TMCP + tempering Yes Same as TMCP Common on thick or E/F plate
Normalized No — Dropped in 2025 for this level
Quenched and tempered Not listed — Use GB/T 16270 if QT is required

Q420q is a TMCP grade with C ≤0.11%, so weldability is judged by Pcm. TMCP + tempering is often used on E and F plate to improve toughness scatter. D-letter plate is usually plain TMCP; tempering is added mainly for heavy plate or tight yield-ratio limits.

Ask for the route on the purchase order. It changes the weldability index, the welding procedure and, for heavy plate, the price of Q420qD.

Welding Q420qD and Fatigue in Bridge Girders

GB/T 714-2025 clause 7.1.2 uses CEV for normalized, QT and TMCP steel with C >0.12%, and Pcm for weathering steel and TMCP steel with C ≤0.12%, both from the heat analysis:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Index ≤50 mm >50–100 mm >100–130 mm
Pcm, TMCP (Table 7) ≤ 0.22 ≤ 0.22 ≤ 0.22

The index caps in GB/T 714 are maximums. Real Q420qD heats often sit well below them, and preheat should be set from the actual value, not the cap. At −20°C, most procedures qualified on TMCP plate pass HAZ impact without special measures; keep multi-wire SAW heat input inside the qualified band.

Typical consumables for Q420qD: E55-class low-hydrogen consumables (AWS E8018 type).

Fatigue. Welded details govern fatigue life in a bridge, and their fatigue strength is set by detail category, not by yield strength. Higher-strength plate can carry higher stress ranges only if detailing improves too.

Fatigue design follows JTG D64 (highway) and TB 10091 (railway) in China, EN 1993-1-9 in Europe and AASHTO LRFD in the US; fabrication commonly follows TB 10212, JTG/T 3650 or AWS D1.5.

Q420qDZ15, Z25 and Z35: Through-Thickness Plate for Bridges

On long-span bridges, Z25 or Z35 is common on node plates and anchor zones. The extra cost is in desulfurization, testing and a higher reject rate.

GB/T 714 adds the Z level to the end of the designation, for example Q420qDZ25. The test and acceptance follow GB/T 5313 and apply to plate 15 mm and thicker.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

D chemistry allows S up to 0.015%. Z15 needs S ≤0.010% and Z25 needs ≤0.007%, so Z plate is still made from a dedicated low-sulfur heat.

Z-grade Q420qD carries a longer lead time because the heat must be planned as low-sulfur from the start. Tell us early. Z options apply across the GB/T 714 bridge steel range.

Equivalent Material Grades

Annex B of GB/T 714-2025 lists foreign grades against each strength level. It is informative: it tells you which families are close, not that the plates are interchangeable.

Standard Grade(s) Fit for Q420qD
EN 10025-4 EN 10025-4 S420M, EN 10025-4 S420ML Listed in Annex B
EN 10025-3 EN 10025-3 S420N, EN 10025-3 S420NL Normalized alternative
ASTM A572 ASTM A572 Gr.60 Strength only, not a bridge grade
GB/T 1591 GB/T 1591 Q420MD General structural
GB/T 714 (weathering twin) Q420qNHD Same strength, weathering chemistry

Before substituting, compare three things line by line: minimum yield at the actual thickness, the impact test temperature and energy, and the weldability index. For Q420qD, the 120 J impact level and the Pcm/CEV caps are usually the hardest to match.

Q420qD Testing, UT and Certificate

A batch of Q420qD is one grade, one heat, one thickness, one rolling schedule and one heat-treatment condition, up to 60 t. Table 12 of GB/T 714-2025 sets the tests:

Test Frequency Method
Heat analysis 1 per heat GB/T 20066; GB/T 4336 / GB/T 223
Tensile 1 per batch GB/T 2975 / GB/T 228.1
Bend 180° 1 per batch (may be waived if guaranteed) GB/T 232
Charpy V at −20°C 3 specimens per batch GB/T 229
Through-thickness (Z) 3 specimens per batch, when ordered GB/T 5313
Ultrasonic Every plate >20 mm, Class II or better GB/T 2970
Surface and dimensions Every plate Visual and gauges

Impact retest: if a set fails, three more specimens are taken from the same batch. The average of all six must meet the requirement; two values may be below it, but only one below 70%. At −20°C the 120 J level is comfortable for well-made TMCP plate, but we still check each batch value, not just the average.

Dimensions

Common Q420qD sizes:

  • Thickness: 6 mm – 130 mm under GB/T 714 tensile tables; most orders 10 – 80 mm
  • Width: 1500 – 4000 mm, depending on mill and thickness
  • Length: 6000 – 18000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, 7.85 g/cm³

Deck plate, webs, flanges, diaphragms and stiffeners are cut to drawing. For U-ribs and rolled sections on the same bridge, see steel beam profiles and steel structural profiles.

Tolerances

Dimensional tolerances for Q420qD follow GB/T 709, as GB/T 714 directs. The default is Class B, which fixes the minus side at 0.30 mm.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Bridge fabricators often ask for Class C (zero minus) on deck and flange plate so section properties are never under the design value. Wider plates follow the heavier GB/T 709 rows; we state them on the offer.

Q420qD Price Factors and How to Order

There is no single Q420qD price. Mills price bridge plate as base plus extras, and the order sets the extras.

Cost driver Effect on price
Strength level Q420q Higher levels need more alloy and tighter rolling control
Quality letter Small extra for −20°C testing and cleaner melt
Delivery route TMCP / TMCP+T
Thickness Over 60 mm and under 10 mm carry size extras
Z15 / Z25 / Z35 Low-sulfur heat, Z test, UT; Z35 costs most
Width and length Over 3000 mm wide or 15 m long needs mill confirmation
Quantity per size Mill minimums per heat and size
Inspection and processing 3.2 witness, profile cutting, blasting, priming quoted per item

To get a firm quote in one round, send:

  • Grade, edition and Z level, e.g. Q420qDZ25 to GB/T 714-2025
  • Thickness × width × length and pieces or tonnes
  • Delivery route and UT class if beyond Class II
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line. Need another letter? See Q420qE, Q420qF.

Applications

Sector Typical Q420qD components
Long-span railway bridges Main truss chords and node plates
Cable-stayed bridges Steel box girders, anchor boxes
Suspension bridges Stiffening girders
Combined road-rail bridges Truss members carrying heavy rail load
Arch bridges Arch ribs and hangers’ anchorages

The letter D suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C.

It is the wrong plate for pressure equipment (pressure vessel steel plates), unpainted exposure (weathering steel plates) or ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q420qD from first-line bridge-plate mills, including drafters of GB/T 714-2025 such as Ansteel, Valin Xiangtan, Jiangyin Xingcheng, Wuyang, Shougang and Xinyu.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness (SGS, BV, TÜV or owner’s inspector)
  • Tests: tensile, −20°C Charpy, bend, Z test, UT, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blasting and priming
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill, per GB/T 247

Our Q420qD exports follow Chinese bridge design abroad: railway and highway bridges built by EPC contractors in Asia, Africa and Latin America.

Lead time: about 30–45 days from mill rolling; Z35, F letter or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Southeast Asia and 28–35 days to North Europe.

Why Choose SHH STEEL

SHH STEEL is a steel manufacturer and exporter and global steel mill sourcing partner. We buy Q420qD mill-direct, China origin, and check every certificate before shipment.

Before shipment we check four lines on every Q420qD certificate: yield and tensile for the actual thickness band, Charpy at −20°C, the CEV or Pcm for the delivery route, and UT results. If one fails, the plate does not ship as Q420qD.

Q420qD is judged by Pcm, not CEV. If your welding specification still sets preheat from CEV, ask us for both values on the certificate.

We also tell buyers when another grade fits better. Neighbouring levels are Q390q and Q460qD. The weathering counterpart is Q420qNHD. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q420qD steel?
Q420qD is bridge structural steel plate to GB/T 714-2025. It has 420 MPa minimum yield up to 50 mm, 540 MPa minimum tensile, 19% elongation and Charpy V-notch impact of 120 J at −20°C for 12–100 mm plate. It is delivered TMCP or TMCP + tempering.
What is the difference between Q420qD and Q420qE?
Strength and chemistry box are the same. Q420qD is Charpy tested at −20°C, Q420qE at −40°C, both needing 120 J for 12–100 mm plate. P/S caps are 0.025/0.015% for D and 0.020/0.010% for E. Choose by the lowest service or erection temperature.
Which bridge first used Q420qE?
The Nanjing Dashengguan Yangtze River Bridge, a six-track railway steel arch bridge, was the first large Chinese bridge to use Q420qE, for its main truss members. The grade has since become common on long-span railway bridges.
What is the ASTM or EN equivalent of Q420qD?
Close grades for Q420qD: EN 10025-4 S420M, S420ML (Annex B) / ASTM A572 Gr.60 (strength only). These are close families, not drop-in substitutes; compare yield at thickness, impact temperature and energy, and the weldability index before substituting.
Is GB/T 714-2015 still valid?
No. GB/T 714-2025 was published on 31 October 2025 and took effect on 1 May 2026, fully replacing GB/T 714-2015. Contracts that still cite the 2015 edition can be certified to it, but new orders default to the 2025 edition.
Is Q420qD weldable?
Yes. GB/T 714-2025 caps the weldability index for Q420qD up to 50 mm at Pcm ≤0.22%. Preheat depends on actual chemistry, thickness and restraint, and is fixed by the qualified welding procedure.

Conclusion

Q420qD to GB/T 714-2025 is bridge plate with 420 MPa minimum yield, 540 MPa minimum tensile and 120 J Charpy at −20°C for 12–100 mm plate.

It sits between Q390q and Q460qD in the bridge range, with Q420qE and Q420qF as sister letters. For Q420qD, a product analysis on finished plate is judged against GB/T 222 deviations, not the heat limits, so put the basis in the contract.

Our Q420qD certificates carry heat chemistry, weldability index, tensile and Charpy data to EN 10204 3.1 or 3.2. SHH STEEL can add product analysis, Z15–Z35 and witness inspection.

We ship from Shanghai to bridge builders worldwide. Browse the full GB/T 714 range or other high strength low alloy plates.

Share your size list, Z level and edition, and we reply with mill, route, lead time, test plan and price in one message. Contact SHH STEEL for a mill-direct Q420qD bridge steel plate quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X