GB/T 714 Q390qNH weathering bridge steel stacked at SHH STEEL warehouse

GB/T 714 Q390qNH Weathering Bridge Steel Supplier

GB/T 714 Q390qNH (Q390qNH) is weathering bridge steel plate with 390 MPa minimum yield, Charpy in C, D or E grade, Cu-Cr-Ni chemistry and a weathering index I ≥6.0 for unpainted bridges. SHH STEEL supplies it mill-direct with Z15–Z35, UT and full heat and product analysis.
Keywords
Q390qNH, Q390qNH weathering steel, GB/T 714 Q390qNH, Q390qNH, Q390qNH steel plate, Q390qNH, Q390qNH weathering bridge steel, Q390qNHZ15, Q390qNHZ25, Q390qNHZ35, bridge steel plate, Q390qNH supplier
Equivalent Grades:
No direct equivalent in Annex B / closest: ASTM A709 HPS 50W / EN 10025-5 S355K2W — Material Specification: GB/T 714-2025 (supersedes GB/T 714-2015) — Delivery: TMCP / TMCP+T
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q390qNH Quality Grades
GB/T 714-2025 vs 2015
Q390qNH vs ASTM A709 / EN 10025
Weathering Index and Unpainted Use
Welding and Fatigue
Z15 / Z25 / Z35
Equivalent Material Grades
Testing and Inspection
Dimensions
Tolerances
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 714 Q390qNH Weathering Bridge Steel?

Q390qNH is weathering bridge structural steel to GB/T 714. In the standard’s own notation it is written Q390qNH: Q for yield, 390 for the minimum yield in MPa, q for qiao (bridge), and NH for nai hou, weathering.

Q390qNH is the new weathering grade added in GB/T 714-2025, giving 390 MPa yield in an unpainted bridge plate. Q390qNH fills the jump between Q370qNH and Q420qNH. It uses the same Cu-Cr-Ni weathering chemistry as Q345qNH with Pcm ≤0.22% to 50 mm, and is tested in C, D or E.

Q390qNH is new in GB/T 714-2025: 390 MPa yield, weathering chemistry, Pcm ≤0.22% to 50 mm, in quality grades C, D or E. It closes the gap between Q370qNH and Q420qNH for unpainted girders.

GB/T 714-2025, in force since 1 May 2026, fully replaces GB/T 714-2015; the changes for weathering grades are listed below.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q390qNH cut to size with an EN 10204 3.1 or 3.2 certificate. Sister grades are listed under GB/T 714; other unpainted options are under weathering steel plates and EN 10025-5.

Material Specification

Specification element Requirement SHH STEEL compliance
Standard GB/T 714-2025 Q390qNH Confirmed
Product Single-rolled plate ≤150 mm; hot-rolled strip and cut plate ≤25.4 mm Plate
Thickness with tensile values Up to 130 mm for Q390qNH Confirmed
Minimum yield ReL 390 MPa ≤50 mm; 380 MPa >50–100 mm Confirmed
Minimum tensile Rm 520 MPa ≤100 mm (no upper limit in the standard) Confirmed
Elongation A ≥ 20% Confirmed
Charpy V-notch C 0°C / D −20°C / E −40°C, 120 J (12–100 mm) Confirmed
Weathering index I ≥ 6.0 (Table 5, footnote c) Calculated on MTC
Delivery condition TMCP or TMCP + tempering As ordered
Weldability index Pcm (Table 8) Printed on MTC
Ultrasonic testing Plate >20 mm: GB/T 2970, Class II or better Every plate
Through-thickness Z15, Z25 or Z35 to GB/T 5313, when ordered As ordered
Dimensions GB/T 709 Confirmed
Certificate GB/T 247; EN 10204 3.1 or 3.2 As ordered

Grades often compared with Q390qNH are ASTM A709 Grade 50W, ASTM A709 HPS 50W and EN 10025-5 S355K2W; the comparison below shows where they differ.

Chemical Composition: Heat Analysis and Product Analysis

Bridge owners increasingly order a product analysis on finished plate. For Q390qNH that check is judged against GB/T 714 heat limits plus the deviations in GB/T 222, not against the heat limits alone.

Table 1 below is the heat (ladle) analysis for Q390qNH from GB/T 714-2025 Tables 1, 5.

Element Q390qNH heat analysis (%) Note
C, max 0.11
Si 0.15 – 0.50 Counts in I
Mn 1.10 – 1.50 Min 0.50% for coil only
P, max 0.030 (C) / 0.025 (D) / 0.020 (E) By letter
S, max 0.025 (C) / 0.015 (D) / 0.010 (E) By letter
Cu 0.25 – 0.50 Main weathering element
Cr 0.40 – 0.70 Weathering element
Ni 0.30 – 0.40 Weathering element
Mo, max 0.20
Nb 0.010 – 0.100 Microalloy (see note)
V 0.010 – 0.100 Microalloy (see note)
Ti 0.006 – 0.030 Microalloy (see note)
Als 0.015 – 0.050 Alt 0.020–0.055% if total Al is used
N, max 0.0080
B, max (residual) 0.0005 ≤0.0014% if C ≤0.06%
H, max (residual) 0.0002
Weathering index I ≥ 6.0 Calculated from heat analysis

Nb, V, Ti and Al may be added singly or together. Added singly, each must meet the range above; added together, at least one must reach its minimum and Nb + V + Ti ≤ 0.22%. Calcium treatment is required to control sulfide shape.

Table 2 is the product analysis: the limits a check analysis on finished plate is judged against. GB/T 714-2025 clause 7.1.3 calls up GB/T 222 for the permitted deviations.

Element Heat limit (%) Deviation, GB/T 222-2025 Table 1 Q390qNH product analysis (%)
C ≤ 0.11 +0.02 ≤ 0.13
Si 0.15 – 0.50 ±0.05 0.10 – 0.55
Mn 1.10 – 1.50 ±0.06 1.04 – 1.56
P ≤ 0.030 (C letter) +0.005 ≤ 0.035
S ≤ 0.025 (C letter) +0.005 ≤ 0.030
V 0.010 – 0.100 +0.02 / −0.01 ≤ 0.120
Ti 0.006 – 0.030 +0.02 / −0.01 ≤ 0.050
Nb 0.010 – 0.100 ±0.005 (listed for 0.015–0.060%) Above 0.060%: agree in contract
Cu 0.25 – 0.50 ±0.05 0.20 – 0.55
Cr 0.40 – 0.70 ±0.05 0.35 – 0.75
Ni 0.30 – 0.40 ±0.05 0.25 – 0.45
Als 0.015 – 0.050 ±0.003 Lower limit −0.003 (Table 1 row is for Al ≥0.015%; confirm)
Mo ≤ 0.20 Not listed in Table 1 Agree in contract
N ≤ 0.0080 Listed only for 0.010–0.020% Agree in contract

How to read Table 2. Weathering bridge steel is normally classed as low-alloy steel, so Table 1 of GB/T 222 applies. Where the heat limit is a range, the deviation applies to both ends; for one heat, an element may deviate in one direction only.

Mechanical Properties

Tensile values follow Table 9 of GB/T 714-2025 for Q390qNH. Tensile specimens are transverse; round specimens are used above 40 mm. Where yield is not distinct, Rp0.2 replaces ReL.

Nominal thickness ReL min (MPa) Rm min (MPa) A min
≤ 50 mm 390 520 20%
> 50 – 100 mm 380 520 20%
> 100 – 130 mm 335 450 20%

Impact values follow Table 10, on longitudinal specimens, average of three:

Letter / test temperature KV2 ≤12 mm KV2 >12 – 100 mm KV2 >100 – 130 mm
C / 0°C 80 J 120 J 55 J
D / −20°C 80 J 120 J 47 J
E / −40°C 80 J 120 J 31 J

One single value may fall below the required average, but not below 70% of it. Plate over 8 mm and under 12 mm is tested with 7.5 mm specimens (75% of the value); 6–8 mm plate with 5 mm specimens (50%). Plate under 6 mm is not impact tested.

180° bend test, transverse: mandrel D = 2a up to 16 mm and 3a above 16 mm; may be omitted when the mill guarantees it. Yield ratio is not mandatory. If the contract asks for it, Annex C recommends ReL/Rm ≤ 0.88 up to 12 mm and ≤ 0.85 above 12 mm for TMCP plate.

Q390qNH C, D or E: Which Quality Grade?

Q390qNH is ordered with a letter. All three share chemistry box, strength and Pcm cap; they differ in test temperature and in P and S limits.

Grade Test temp. KV2 ≤12 mm KV2 12–100 mm KV2 >100 mm P / S max (%)
Q390qCNH 0°C 80 J 120 J 55 J 0.030 / 0.025
Q390qDNH −20°C 80 J 120 J 47 J 0.025 / 0.015
Q390qENH −40°C 80 J 120 J 31 J 0.020 / 0.010

Pick C for sites that stay near or above 0°C, D for winters down to about −20°C, and E for colder sites or thick, restrained members. There is no F letter at the 390 MPa level; for −60°C look at Q420qNHF.

Neighbouring grades: Q370qNHD below and Q420qNHD above.

Q390qNH: What Changed from GB/T 714-2015 to GB/T 714-2025

For Q390qNH buyers the 2025 edition changes more than the year on the certificate. The points below come from the foreword of GB/T 714-2025 and its tables.

  • Q390qNH is a new grade; it did not exist in GB/T 714-2015.
  • The weathering requirement changed: Table 5 now requires a corrosion index I ≥ 6.0, and the 2015 Annex C guide for assessing weathering resistance was deleted.
  • A Pcm table for weathering steel (Table 8) was added.
  • Annex A now gives reference bridge-site environments for unpainted use (chloride, SO₂ and time-of-wetness limits).
  • Tensile strength is now banded by thickness (e.g. lower minimum Rm above 100 mm) instead of one value.
  • Impact energy is set by thickness band (≤12 mm, 12–100 mm, >100 mm) in Table 10.
  • Yield ratio is no longer a clause value; it is agreed in the contract, with recommendations in informative Annex C.

If a drawing cites 2015 and the plate is made to 2025, get the designer’s written acceptance; tensile strength above 100 mm and the yield-ratio basis differ.

Q390qNH vs ASTM A709 and EN 10025: Which Grade Matches?

Can Q390qNH replace a US or European bridge grade, or the other way round? Strength can match; toughness rules differ in kind, not only in number.

Property Q390qNH ASTM A709 Grade 50W ASTM A709 HPS 50W EN 10025-5 S355K2W
Min. yield (MPa) 390 (≤50 mm) 345 345 355 (≤16 mm)
Tensile (MPa) 520 min 485 min 485 min 470 – 630
Charpy 120 J at 0 / −20 / −40°C (C/D/E) CVN by temperature zone and member type (T / F) CVN by temperature zone; fracture-critical (F) levels 40 J at −20°C
Weathering chemistry Yes, I ≥ 6.0 Yes Yes Yes

ASTM A709 sets Charpy requirements by temperature zone (1, 2, 3) and by member type: non-fracture-critical (T) or fracture-critical (F). GB/T 714 sets one value per letter, so compare the A709 zone with the GB/T 714 test temperature, not grade with grade.

EN 10025-5 weathering grades are general structural steels without a bridge-specific toughness level of 120 J; they suit many bridges but are not a one-to-one match.

The 120 J requirement for 12–100 mm plate is several times the 27–40 J typical of general weathering grades such as ASTM A588 or Corten A/B plate, which is why bridge owners specify Q390qNH.

Q390qNH Atmospheric Corrosion Index I and Unpainted Bridges

GB/T 714-2025 Table 5, footnote c, requires every Q390qNH heat to reach an atmospheric corrosion index I of at least 6.0, calculated from the heat analysis:

I = 26.01(%Cu) + 3.88(%Ni) + 1.20(%Cr) + 1.49(%Si) + 17.28(%P) − 7.29(%Cu)(%Ni) − 9.10(%Ni)(%P) − 33.39(%Cu)²

This is the same predictive formula used with ASTM G101 for ASTM A709 Grade 50W and ASTM A709 HPS 70W, which makes Chinese and US ASTM A709 weathering steel plates easy to compare with Q390qNH.

Worked example (our calculation) Cu Ni Cr Si P I
All weathering elements at their Table 5 minimum 0.25 0.30 0.40 0.15 0.010 5.88
Illustrative mid-range heat 0.32 0.36 0.55 0.30 0.012 6.74

Note the first row: a heat that only just meets every Table 5 minimum can still fall short of I = 6.0. That is why we ask the mill to print I on every Q390qNH certificate, not just the chemistry.

Where can the steel be left unpainted? Annex A of GB/T 714-2025 gives reference bridge-site conditions:

  • Rural or urban atmosphere with annual chloride deposition ≤ 3 mg/(m²·d)
  • Annual SO₂ deposition ≤ 24 mg/(m²·d)
  • Time of wetness ≤ 5,256 h per year (temperature above 0°C and relative humidity above 80%)
  • Coastal sites only if they meet the same limits; for marine atmospheres Annex D points to T/CISA 073

Weathering steel is not stainless. Q390qNH corrodes slowly once a stable patina forms, which takes a few years of wet-dry cycles. Designers usually add a corrosion allowance and design drainage so no surface stays wet.

Welding Q390qNH and Fatigue in Bridge Girders

GB/T 714-2025 clause 7.1.2 uses CEV for normalized, QT and TMCP steel with C >0.12%, and Pcm for weathering steel and TMCP steel with C ≤0.12%, both from the heat analysis:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Index ≤50 mm >50–100 mm >100–130 mm
Pcm, Q390qNH (Table 8) ≤ 0.22 ≤ 0.24 By agreement

We send the actual heat analysis of Q390qNH before shipment, so the fabricator can check preheat and interpass limits against the procedure qualification record.

Typical consumables for Q390qNH: weathering-matched Ni-Cu consumables (AWS E8018-W2 type for 345–420 MPa), with higher-strength weathering wires for 460–500 MPa.

Fatigue. Welded details govern fatigue life in a bridge, and their fatigue strength is set by detail category, not by yield strength. Higher-strength plate can carry higher stress ranges only if detailing improves too.

Fatigue design follows JTG D64 (highway) and TB 10091 (railway) in China, EN 1993-1-9 in Europe and AASHTO LRFD in the US; fabrication commonly follows TB 10212, JTG/T 3650 or AWS D1.5.

Q390qNHZ15, Z25 and Z35: Through-Thickness Plate for Bridges

When a bridge drawing marks a plate Z25, the mill must supply a low-sulfur heat and prove reduction of area through the thickness on every batch.

GB/T 714 adds the Z level to the end of the designation, for example Q390qNHZ25. The test and acceptance follow GB/T 5313 and apply to plate 15 mm and thicker.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

Q390q C-letter plate allows S up to 0.025%, D 0.015% and E 0.010%; only E meets the Z15 sulfur cap without a dedicated heat.

For Q390qNH, we test Z per GB/T 5313 batch rules and print the three reduction-of-area values on the certificate. Z options apply across the GB/T 714 bridge steel range.

Equivalent Material Grades

Annex B of GB/T 714-2025 lists foreign grades against each strength level. It is informative: it tells you which families are close, not that the plates are interchangeable.

Standard Grade(s) Fit for Q390qNH
ASTM A709 ASTM A709 Grade 50W, ASTM A709 HPS 50W Closest; lower yield
EN 10025-5 EN 10025-5 S355K2W Closest; lower yield
ASTM A588 ASTM A588 Grade C Similar chemistry family
GB/T 714 (painted twin) Q390q Same strength, no weathering elements

For weathering grades also compare the corrosion index basis. Q390qNH requires I ≥ 6.0 by the formula above; check that the substitute is assessed on the same basis.

Q390qNH Testing, UT and Certificate

A batch of Q390qNH is one grade, one heat, one thickness, one rolling schedule and one heat-treatment condition, up to 60 t. Table 12 of GB/T 714-2025 sets the tests:

Test Frequency Method
Heat analysis 1 per heat GB/T 20066; GB/T 4336 / GB/T 223
Weathering index I Calculated per heat Table 5 formula
Tensile 1 per batch GB/T 2975 / GB/T 228.1
Bend 180° 1 per batch (may be waived if guaranteed) GB/T 232
Charpy V at the ordered letter’s temperature 3 specimens per batch GB/T 229
Through-thickness (Z) 3 specimens per batch, when ordered GB/T 5313
Ultrasonic Every plate >20 mm, Class II or better GB/T 2970
Surface and dimensions Every plate Visual and gauges

Impact retest: if a set fails, three more specimens are taken from the same batch. The average of all six must meet the requirement; two values may be below it, but only one below 70%.

Dimensions

Common Q390qNH sizes:

  • Thickness: 6 mm – 130 mm under GB/T 714 tensile tables; most orders 8 – 60 mm
  • Width: 1500 – 4000 mm, depending on mill and thickness
  • Length: 6000 – 18000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, 7.85 g/cm³

Deck plate, webs, flanges, diaphragms and stiffeners are cut to drawing. For U-ribs and rolled sections on the same bridge, see steel beam profiles and steel structural profiles.

Tolerances

GB/T 714-2025 clause 7.6 sends dimensions and shape to GB/T 709. Thickness tolerance is Class B by default: −0.30 mm fixed, plus side by thickness and width.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Bridge fabricators often ask for Class C (zero minus) on deck and flange plate so section properties are never under the design value. Wider plates follow the heavier GB/T 709 rows; we state them on the offer.

Q390qNH Price Factors and How to Order

Bridge plate prices move with the steel market, but for Q390qNH the order details often matter more.

Cost driver Effect on price
Strength level Q390q Higher levels need more alloy and tighter rolling control
Quality letter C < D < E; letter chosen on order
Weathering alloys Cu, Cr, Ni additions and I-index control add a weathering extra
Delivery route TMCP / TMCP+T
Thickness Over 60 mm and under 10 mm carry size extras
Z15 / Z25 / Z35 Low-sulfur heat, Z test, UT; Z35 costs most
Width and length Over 3000 mm wide or 15 m long needs mill confirmation
Quantity per size Mill minimums per heat and size
Inspection and processing 3.2 witness, profile cutting, blasting, priming quoted per item

To get a firm quote in one round, send:

  • Grade, edition and Z level, e.g. Q390qDNHZ25 to GB/T 714-2025
  • Thickness × width × length and pieces or tonnes
  • Delivery route and UT class if beyond Class II
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line, so offers can be compared like for like.

Applications

Sector Typical Q390qNH components
Unpainted highway bridges Plate girders and box girders in rural and urban atmospheres
Railway bridges Truss members, plate girders, bracing
Remote and mountain sites Bridges where repainting access is difficult or costly
Urban viaducts Exposed girders with architectural rust finish
Pedestrian bridges Unpainted box sections

The C/D/E choice suits bridges from warm to cold climates, chosen by letter.

Q390qNH is the wrong plate for marine splash zones, tunnels, sites with heavy de-icing salt spray, or members that stay wet. There, use painted Q390q or look at marine-atmosphere grades under T/CISA 073.

Supply Capability and Global Delivery

SHH STEEL sources Q390qNH from first-line bridge-plate mills, including drafters of GB/T 714-2025 such as Ansteel, Valin Xiangtan, Jiangyin Xingcheng, Wuyang, Shougang and Xinyu.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness (SGS, BV, TÜV or owner’s inspector)
  • Tests: tensile, C/D/E Charpy, bend, Z test, UT, product analysis, weathering index
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blasting and priming (or blasting only, for unpainted weathering steel)
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill, per GB/T 247

Q390qNH leaves Shanghai for bridge projects designed to Chinese codes abroad, mainly through EPC contractors in Southeast Asia, Central Asia, the Middle East and Africa.

Lead time: about 30–45 days from mill rolling; Z35, F letter or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Southeast Asia and 28–35 days to North Europe.

Why Choose SHH STEEL

SHH STEEL has supplied bridge plate as a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. Q390qNH is ordered from mills that roll bridge steel every month.

Before shipment we check four lines on every Q390qNH certificate: yield and tensile for the actual thickness band, Charpy at the ordered letter, the Pcm and weathering index, and UT results. If one fails, the plate does not ship as Q390qNH.

Because the grade is new, fabricators may not have procedures for it. We supply trial-heat chemistry and mechanical data early so qualification can start before the main order.

We also tell buyers when another grade fits better. Neighbouring levels are Q370qNHE and Q420qNHE. The painted counterpart is Q390q. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q390qNH steel?
Q390qNH is a weathering bridge steel added in GB/T 714-2025. It has 390 MPa minimum yield up to 50 mm, 520 MPa minimum tensile, Cu-Cr-Ni weathering chemistry with corrosion index I ≥6.0, Pcm ≤0.22% to 50 mm, and is ordered as Q390qCNH, Q390qDNH or Q390qENH.
What is the difference between Q390qC, Q390qD and Q390qE weathering grades?
Only the impact test temperature and the P and S limits. C is tested at 0°C, D at −20°C and E at −40°C, all requiring 120 J for 12–100 mm plate. P/S caps are 0.030/0.025% for C, 0.025/0.015% for D and 0.020/0.010% for E.
Why was Q390q added to GB/T 714?
GB/T 714-2025 added Q390q to fill the jump from Q370q to Q420q. It keeps the C ≤0.14% TMCP chemistry of Q345q and Q370q with a CEV cap of 0.41%, so designers gain 390 MPa yield without moving to the leaner Q420q chemistry family.
What is the ASTM or EN equivalent of Q390qNH?
Close grades for Q390qNH: No direct equivalent in Annex B / closest: ASTM A709 HPS 50W / EN 10025-5 S355K2W. These are close families, not drop-in substitutes; compare yield at thickness, impact temperature and energy, and the weldability index before substituting.
What is the batch size for GB/T 714 bridge plate testing?
Up to 60 t of one grade, heat, thickness, rolling schedule and heat-treatment condition. Each batch gets one tensile test, one bend test and one set of three Charpy specimens; heat analysis is reported per heat.
What is the weathering index I in GB/T 714?
It is a corrosion index calculated from the heat analysis: I = 26.01Cu + 3.88Ni + 1.20Cr + 1.49Si + 17.28P − 7.29Cu·Ni − 9.10Ni·P − 33.39Cu². GB/T 714-2025 requires I ≥6.0 for every weathering grade, the same basis ASTM G101 uses for A709 weathering steels.

Conclusion

Q390qNH to GB/T 714 is weathering bridge steel with 390 MPa minimum yield, Cu-Cr-Ni chemistry, a weathering index of at least 6.0 and Charpy in C, D or E grade.

It sits between Q370q (C, D, E) and Q420q (D, E, F) in the weathering range, filling the 390 MPa step that GB/T 714-2015 did not have. Before ordering Q390qNH, confirm the edition on the drawing, the delivery route and any Z level; those three choices drive cost, lead time and welding.

Our Q390qNH certificates carry heat chemistry, weldability index, tensile and Charpy data to EN 10204 3.1 or 3.2. SHH STEEL can add product analysis, Z15–Z35 and witness inspection.

We ship from Shanghai to bridge builders worldwide. Browse the full GB/T 714 range or other weathering steel plates.

Send the edition, quality letter, Z level and size list; we confirm mill, delivery route, lead time and price in one reply. Contact SHH STEEL for a mill-direct quotation on Q390qNH weathering bridge steel.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X