EN 10025-4 S420ML Steel Plate | S420ML Fine Grain Structural Steel - SHH STEEL

EN 10025-4 S420ML Steel Plate | S420ML Fine Grain Structural Steel

EN 10025-4 S420ML is a thermomechanically rolled fine-grain structural steel plate with a minimum yield strength of 420 MPa and impact tested at –50°C. It offers high strength, excellent low-temperature toughness and good weldability. SHH STEEL is a China Mill-Direct Exporter supplying S420ML steel plate worldwide.
Equivalent Grades:
ASTM A572 Gr 60 (TMCP, -50℃ CVN) / JIS SM520C (L ref) / GB Q420ME / ISO E420ML
Material Specification:
EN 10025-4 — Delivery: Thermo-Mechanically Rolled (TMCP), -50℃ impact guaranteed
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Tolerances
Weldability
Equivalent Material Grades
Applications
Why Choose SHH STEEL
FAQ
Conclusion

What is EN 10025-4 S420ML Steel Plate?

As a professional steel plate supplier and China Mill-Direct Exporter, SHH STEEL is pleased to present EN 10025-4 S420ML Steel Plate (Material Number: 1.8836).

S420ML is a thermomechanically rolled (TMCP) weldable fine-grain structural steel under the European standard EN 10025-4. It provides a minimum yield strength of 420 MPa (for thickness ≤ 16 mm) and is impact tested at –50°C with a minimum energy of 27 J. Compared with S420M, S420ML offers superior low-temperature toughness, making it suitable for high-strength structural applications in cold environments. SHH STEEL sources this material directly from leading Chinese steel mills, ensuring competitive mill-direct pricing, stable quality and reliable delivery.

We supply S420ML steel plate in thicknesses from 6 mm to 120 mm (thicker plates available on request), widths up to 3000–4000 mm, and lengths up to 12000–18000 mm. Custom cutting, shot blasting and priming services are available. All plates are delivered with full Mill Test Certificates (EN 10204 3.1).

Material Specification

EN 10025-4 S420ML steel plate is produced in accordance with EN 10025-4.

Specification Element Requirement SHH STEEL Compliance
Primary Standard EN 10025-4 Full compliance
Steel Grade S420ML (1.8836) Confirmed
Delivery Condition Thermomechanically rolled (M) Confirmed
Product Form Steel Plate Available
Thickness Range 6 mm – 120 mm Custom sizes available
Width / Length Up to 3000–4000 mm / 12000–18000 mm Custom cutting supported
Certification EN 10204 3.1 / 3.2 Available

Chemical Composition

According to EN 10025-4, the chemical composition is specified for both ladle analysis (cast analysis) and product analysis.

Ladle Analysis (Cast Analysis)

Element Max. / Range (%)
Carbon (C) ≤ 0.16
Silicon (Si) ≤ 0.50
Manganese (Mn) ≤ 1.70
Phosphorus (P) ≤ 0.025
Sulfur (S) ≤ 0.020
Niobium (Nb) ≤ 0.05
Vanadium (V) ≤ 0.12
Aluminium (Al total) ≥ 0.020
Titanium (Ti) ≤ 0.05
Chromium (Cr) ≤ 0.30
Nickel (Ni) ≤ 0.80
Molybdenum (Mo) ≤ 0.20
Copper (Cu) ≤ 0.55
Nitrogen (N) ≤ 0.025

Product Analysis

Element Max. / Range (%)
Carbon (C) ≤ 0.18
Silicon (Si) ≤ 0.55
Manganese (Mn) ≤ 1.80
Phosphorus (P) ≤ 0.030
Sulfur (S) ≤ 0.025
Niobium (Nb) ≤ 0.06
Vanadium (V) ≤ 0.14
Aluminium (Al total) ≥ 0.015
Titanium (Ti) ≤ 0.06
Chromium (Cr) ≤ 0.35
Nickel (Ni) ≤ 0.85
Molybdenum (Mo) ≤ 0.23
Copper (Cu) ≤ 0.60
Nitrogen (N) ≤ 0.027

Note:

  • The minimum Al content does not apply if sufficient other nitrogen-binding elements are present.
  • Carbon Equivalent (CEV) is controlled to ensure good weldability.

Mechanical Properties

Mechanical properties of EN 10025-4 S420ML (longitudinal direction):

Thickness (mm) Yield Strength ReH (min) Tensile Strength Rm Elongation A (min) Impact Energy KV (min)
≤ 16 420 MPa 520 – 680 MPa 19% 27 J at –50°C
> 16 ≤ 40 400 MPa 520 – 680 MPa 19% 27 J at –50°C
> 40 ≤ 63 390 MPa 500 – 660 MPa 19% 27 J at –50°C
> 63 ≤ 80 380 MPa 480 – 640 MPa 19% 27 J at –50°C
> 80 ≤ 100 370 MPa 470 – 630 MPa 19% 27 J at –50°C
> 100 ≤ 120 365 MPa 460 – 620 MPa 19% 27 J at –50°C

Density: 7.85 g/cm³

Delivery Conditions

SHH STEEL, as a China Mill-Direct Supplier, supplies EN 10025-4 S420ML steel plate in the thermomechanically rolled (M) condition.

Additional options:

  • Shot blasting and shop primer
  • Ultrasonic testing (EN 10160)
  • Z-direction testing (Z15 / Z25 / Z35)
  • Third-party inspection (SGS, BV, TUV, etc.)

Tolerances

Dimensional tolerances for S420ML steel plate follow EN 10029 (for plates).

  • Thickness, width and length tolerances according to the ordered class.
  • Flatness according to EN 10029.
  • Edge conditions: Mill edge or cut edge (flame / plasma).

Tighter tolerances can be provided upon request.

Weldability

S420ML has good weldability for a higher-strength thermomechanically rolled fine-grain steel. It can be welded by conventional methods (SMAW, GMAW, FCAW, SAW).

Recommended welding consumables:

Welding Process Recommended Consumables
SMAW (Stick) E7018, E8018
GMAW (MIG/MAG) ER70S-6, ER80S-D2
FCAW E71T-1, E81T1
SAW EM12K / EH14 + suitable flux

Preheating may be required for thicker plates. Low-hydrogen consumables and controlled heat input are recommended, especially for low-temperature service.

Equivalent Material Grades

Grade Standard Notes
S420ML EN 10025-4 —
1.8836 EN Material number
Q420ML / Q420ME GB/T 1591 Closest Chinese equivalents
A572 Grade 60 / A633 (approx.) ASTM Similar strength / toughness concept
TStE 420 TM DIN (old) Former designation

Applications

EN 10025-4 S420ML is used in structural applications requiring high strength and excellent low-temperature toughness. Typical uses include:

Application Area Typical Components / Uses (Keywords)
Building Structures Heavy beams, columns in cold regions – S420ML Structural Steel
Bridges Bridge components – S420ML Bridge
Offshore & Marine Structural components – S420ML Offshore
Machinery Heavy equipment frames – S420ML Machinery
Low-Temperature Construction High-strength structures requiring –50°C toughness – S420ML Construction
General Fabrication Critical welded fine-grain structures – S420ML Fabrication

Why Choose SHH STEEL

SHH STEEL is a China Mill-Direct Exporter. We maintain long-term strategic cooperation with major Chinese steel mills and act as a first-level (primary) agent. This direct mill supply model allows us to offer competitive mill-direct pricing, faster delivery times, stable and traceable quality, and full Mill Test Certificates (EN 10204 3.1 / 3.2) for EN 10025-4 S420ML Steel Plate.

Customers benefit from reliable supply, short lead times and cost-effective solutions for high-strength thermomechanically rolled fine-grain low-temperature structural steel projects worldwide. Our professional export team provides technical support and customized processing services to meet project requirements.

FAQ

What does the “ML” in S420ML mean?
“M” indicates thermomechanically rolled condition, and “L” indicates impact tested at –50°C with a minimum of 27 J.
What is the difference between S420M and S420ML?
Both are thermomechanically rolled. S420M is impact tested at –20°C (40 J), while S420ML is impact tested at –50°C (27 J), providing better low-temperature toughness.
Is S420ML suitable for low-temperature high-strength applications?
Yes. With a minimum yield strength of 420 MPa and guaranteed impact toughness at –50°C, S420ML is ideal for demanding structural applications in cold environments.

Conclusion

EN 10025-4 S420ML (1.8836) Steel Plate from SHH STEEL is a thermomechanically rolled fine-grain structural steel offering high strength (420 MPa) and excellent toughness at –50°C. As a China Mill-Direct Exporter, we provide competitive pricing, fast delivery and consistent quality backed by full mill certifications. Trust SHH STEEL for your S420ML fine grain structural steel plate requirements.

Contact SHH STEEL today for stock availability, pricing and technical support. EN 10025-4 S420ML Steel Plate, S420ML steel plate, S420ML fine grain structural steel, EN 10025 S420ML, S420ML equivalent, S420ML supplier, 1.8836

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X