GB/T 714 Q550qE Bridge Steel Plate Supplier
What is GB/T 714 Q550qE Bridge Steel Plate?
Q550qE is bridge structural steel plate to GB/T 714. Q stands for yield, 550 is the minimum yield in MPa for plate up to 50 mm, q stands for qiao (bridge) and E is the quality grade: Charpy V-notch at −40°C on longitudinal specimens.
Q550q is ultra-high-strength bridge plate up to 100 mm, now available TMCP as well as QT under GB/T 714-2025. Q550q was a QT-only grade in the 2015 edition. The 2025 edition adds a TMCP route with C ≤0.11% and Pcm ≤0.23% to 50 mm, which makes thinner, easier-to-weld plate possible at 550 MPa.
Q550qE combines 550 MPa yield with 120 J at −40°C (12–100 mm). It suits highly stressed truss chords and anchor zones on long-span bridges in cold climates.
Since 1 May 2026, the valid edition is GB/T 714-2025, which fully replaced GB/T 714-2015. The changes matter for buyers: tensile strength now drops by thickness band, impact energy is set by thickness, and the yield ratio moved to an informative annex.
SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q550qE cut to size with an EN 10204 3.1 or 3.2 certificate. Sister grades are listed under GB/T 714.
Material Specification
| Specification element | Requirement | SHH STEEL compliance |
|---|---|---|
| Standard | GB/T 714-2025 Q550qE | Confirmed |
| Product | Single-rolled plate ≤150 mm; hot-rolled strip and cut plate ≤25.4 mm | Plate |
| Thickness with tensile values | Up to 100 mm for Q550q | Confirmed |
| Minimum yield ReL | 550 MPa ≤50 mm; 530 MPa >50–100 mm | Confirmed |
| Minimum tensile Rm | 660 MPa ≤100 mm (no upper limit in the standard) | Confirmed |
| Elongation A | ≥ 16% | Confirmed |
| Charpy V-notch | −40°C, 120 J (12–100 mm), longitudinal | Confirmed |
| Delivery condition | TMCP, TMCP + tempering, or quenched and tempered (QT) | As ordered |
| Weldability index | Pcm (Table 7) for TMCP; CEV (Table 6) for QT | Printed on MTC |
| Ultrasonic testing | Plate >20 mm: GB/T 2970, Class II or better | Every plate |
| Through-thickness | Z15, Z25 or Z35 to GB/T 5313, when ordered | As ordered |
| Dimensions | GB/T 709 | Confirmed |
| Certificate | GB/T 247; EN 10204 3.1 or 3.2 | As ordered |
Grades often compared with Q550qE are and EN 10025-6 S460Q; the comparison below shows where they differ.
Chemical Composition: Heat Analysis and Product Analysis
A check analysis on finished plate often reads a few hundredths higher than the mill certificate. That is not automatically a failure. The certificate shows the heat (ladle) analysis; plate drilled after rolling is judged as product analysis, with the tolerances of GB/T 222.
Table 1 below is the heat (ladle) analysis for Q550qE from GB/T 714-2025 Tables 1, 2, 3 and 4.
| Element | Q550qE TMCP (%) | Q550q quenched and tempered (%) |
|---|---|---|
| C, max | 0.11 | 0.12 |
| Si, max | 0.50 | 0.55 |
| Mn | 0.80 – 1.70 | 0.80 – 1.70 |
| P, max | 0.020 | 0.020 |
| S, max | 0.010 | 0.010 |
| Nb | 0.005 – 0.090 | 0.005 – 0.060 |
| V | 0.010 – 0.080 | 0.010 – 0.080 |
| Ti | 0.006 – 0.030 | 0.006 – 0.030 |
| Als | 0.010 – 0.045 | 0.010 – 0.045 |
| Cr, max | 1.00 | ≤ 0.80 |
| Ni, max | 1.20 | ≤ 0.70 |
| Cu, max | 0.55 | ≤ 0.30 |
| Mo, max | 0.60 | ≤ 0.30 |
| N, max | 0.0080 | 0.0080 |
| B, max | 0.0005 residual (≤0.0014 if C ≤0.10%) | 0.0005–0.0030 may be added |
| H, max | 0.0002 | 0.0002 |
Nb, V, Ti and Al may be added singly or together. Added singly, each must meet the range above; added together, at least one must reach its minimum and Nb + V + Ti ≤ 0.22%.
Table 2 is the product analysis: the limits a check analysis on finished plate is judged against. GB/T 714-2025 clause 7.1.3 calls up GB/T 222 for the permitted deviations.
| Element | Heat limit (%) | Deviation, GB/T 222-2025 Table 2 (alloy) | Q550qE product analysis (%) |
|---|---|---|---|
| C | ≤ 0.11 | +0.01 | ≤ 0.12 |
| Si | ≤ 0.50 | +0.04 | ≤ 0.54 |
| Mn | 0.80 – 1.70 | ±0.04 | 0.76 – 1.74 |
| P | ≤ 0.020 | +0.005 (see note) | ≤ 0.025 |
| S | ≤ 0.010 | +0.005 (see note) | ≤ 0.015 |
| Cr | ≤ 1.00 | +0.05 (0.90–2.10% band) | ≤ 1.05 |
| Ni | ≤ 1.20 | +0.05 (1.00–2.00% band) | ≤ 1.25 |
| Cu | ≤ 0.55 | +0.03 | ≤ 0.58 |
| Mo | ≤ 0.60 | +0.02 (0.30–0.60% band) | ≤ 0.62 |
| V | 0.010 – 0.080 | +0.01 (≤0.10% band) | ≤ 0.090 |
| Ti | 0.006 – 0.030 | +0.02 | ≤ 0.050 |
| Nb, B, N | See heat table | Not read in our copy of Table 2 | Agree in contract |
How to read Table 2. With Ni up to 1.20% and Mo up to 0.60%, Q550q heats are normally classed as alloy steel under GB/T 13304, so the alloy-steel table of GB/T 222 applies. One steel uses one table only; the certificate should say which.
Mechanical Properties
Tensile values follow Table 9 of GB/T 714-2025 for Q550q. Tensile specimens are transverse; round specimens are used above 40 mm. Where yield is not distinct, Rp0.2 replaces ReL.
| Nominal thickness | ReL min (MPa) | Rm min (MPa) | A min |
|---|---|---|---|
| ≤ 50 mm | 550 | 660 | 16% |
| > 50 – 100 mm | 530 | 660 | 16% |
Impact values follow Table 10, on longitudinal specimens, average of three:
| Letter / test temperature | KV2 ≤12 mm | KV2 >12 – 100 mm | KV2 >100 – 150 mm |
|---|---|---|---|
| E / −40°C | 80 J | 120 J | Not applicable |
One single value may fall below the required average, but not below 70% of it. Plate over 8 mm and under 12 mm is tested with 7.5 mm specimens (75% of the value); 6–8 mm plate with 5 mm specimens (50%). Plate under 6 mm is not impact tested.
180° bend test, transverse: mandrel D = 2a up to 16 mm and 3a above 16 mm; may be omitted when the mill guarantees it. Yield ratio is not mandatory and Annex C gives no recommended value at this level; agree a limit in the contract if the design needs one.
Q550qD / Q550qE / Q550qF: Which Quality Grade?
Q550qE is tested at −40°C. It suits bridges in north-east China, Inner Mongolia, Xinjiang, Russia, Kazakhstan, Canada and high-altitude sites, and for thick, restrained members anywhere. E is tested at −40°C, with P ≤0.020% and S ≤0.010%. Many long-span bridges specify E even in mild climates, because thick plate and heavy welding raise the risk of brittle fracture.
| Grade | Test temp. | KV2 ≤12 mm | KV2 12–100 mm | KV2 >100 mm | P / S max (%) |
|---|---|---|---|---|---|
| Q550qD | −20°C | 80 J | 120 J | — | 0.025 / 0.015 |
| Q550qE | −40°C | 80 J | 120 J | — | 0.020 / 0.010 |
| Q550qF | −60°C | By agreement | 60 J | — | 0.015 / 0.006 |
Over-specifying the letter costs money; under-specifying it costs safety. Choose from the lowest service or erection temperature, then step up one letter for thick, restrained or fracture-critical members.
Q550qE: What Changed from GB/T 714-2015 to GB/T 714-2025
For Q550qE buyers the 2025 edition changes more than the year on the certificate. The points below come from the foreword of GB/T 714-2025 and its tables.
- A TMCP route was added for Q550q (C ≤0.11%, Pcm ≤0.23% to 50 mm). In 2015 it was QT only.
- CEV and Pcm limits were revised (Tables 6 and 7).
- Tensile strength is now banded by thickness (e.g. lower minimum Rm above 100 mm) instead of one value.
- Impact energy is set by thickness band (≤12 mm, 12–100 mm, >100 mm) in Table 10.
- Yield ratio is no longer a clause value; it is agreed in the contract, with recommendations in informative Annex C.
- Section products were removed; the standard now covers plate and strip only.
- Delivery is TMCP, TMCP + tempering or QT; normalizing is kept only for Q345q/Q370q plate over 100 mm by agreement.
If a drawing cites 2015 and the plate is made to 2025, get the designer’s written acceptance; tensile strength above 100 mm and the yield-ratio basis differ.
Q550qE vs ASTM A709 and EN 10025: Which Grade Matches?
Can Q550qE replace a US or European bridge grade, or the other way round? Strength can match; toughness rules differ in kind, not only in number.
| Property | Q550qE | EN 10025-6 S460Q | EN 10025-6 S550Q |
|---|---|---|---|
| Min. yield (MPa) | 550 (≤50 mm) | 460 (≤50 mm) | 550 (≤50 mm) |
| Tensile (MPa) | 660 min | 550 – 720 | 640 – 820 |
| Charpy | 120 J at −40°C (12–100 mm) | Q: −20°C, QL: −40°C, QL1: −60°C | Q / QL / QL1: −20 / −40 / −60°C |
| Weathering chemistry | No | No | No |
ASTM A709 sets Charpy requirements by temperature zone (1, 2, 3) and by member type: non-fracture-critical (T) or fracture-critical (F). GB/T 714 sets one value per letter, so compare the A709 zone with the GB/T 714 test temperature, not grade with grade.
EN 10025-3/-4/-6 grades show yield at the thinnest band; their values fall with thickness. GB/T 714 keeps 550 MPa to 50 mm. EN tensile ranges have upper limits; GB/T 714 gives minimums only.
The 120 J requirement in GB/T 714 for 12–100 mm plate is several times the 27–40 J typical of general structural grades. That margin is the main reason bridge owners specify Q550qE rather than GB/T 1591 plate.
Q550qE Delivery Condition: TMCP vs Normalized vs Quenched and Tempered
GB/T 714-2025 clause 3.2 defines TMCP as rolling with the final deformation in a controlled temperature range, including accelerated cooling with or without tempering (self-tempering included) but excluding direct quenching and quench-and-temper. The delivery route must be stated on the certificate.
| Route | Available for Q550qE | Weldability index | Notes |
|---|---|---|---|
| TMCP | Yes | Pcm ≤0.23% (≤50 mm) | C ≤0.11%; up to 100 mm |
| TMCP + tempering | Yes | Pcm | Improves toughness uniformity |
| Quenched and tempered | Yes | CEV ≤0.52% (≤50 mm) | C ≤0.12%; B 0.0005–0.0030% may be added |
| Normalized | No | — | Not listed |
Before 2026, Q550q bridge plate was QT only. GB/T 714-2025 added TMCP, which allows leaner chemistry and easier welding on plate up to about 50 mm. For E-letter plate over about 50 mm, many mills add tempering after TMCP to reduce toughness scatter through the thickness.
Ask for the route on the purchase order. It changes the weldability index, the welding procedure and, for heavy plate, the price of Q550qE.
Welding Q550qE and Fatigue in Bridge Girders
GB/T 714-2025 clause 7.1.2 uses CEV for normalized, QT and TMCP steel with C >0.12%, and Pcm for weathering steel and TMCP steel with C ≤0.12%, both from the heat analysis:
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B
| Index | ≤50 mm | >50–100 mm | >100–130 mm |
|---|---|---|---|
| Pcm, TMCP (Table 7) | ≤ 0.23 | ≤ 0.25 | — |
| CEV, QT (Table 6) | ≤ 0.52 | ≤ 0.57 | — |
Most bridge fabricators qualify Q550qE procedures on plate from the same mill and route as the production order. Changing mill or route mid-project usually means re-qualifying. At −40°C, HAZ toughness often becomes the limit. Fabricators usually cap heat input and qualify the procedure at −40°C on plate from the same route.
Typical consumables for Q550qE: E62/E69-class consumables (AWS E9018M / E10018M type).
Fatigue. Welded details govern fatigue life in a bridge, and their fatigue strength is set by detail category, not by yield strength. Higher-strength plate can carry higher stress ranges only if detailing improves too.
Fatigue design follows JTG D64 (highway) and TB 10091 (railway) in China, EN 1993-1-9 in Europe and AASHTO LRFD in the US; fabrication commonly follows TB 10212, JTG/T 3650 or AWS D1.5.
Q550qEZ15, Z25 and Z35: Through-Thickness Plate for Bridges
On long-span bridges, Z25 or Z35 is common on node plates and anchor zones. The extra cost is in desulfurization, testing and a higher reject rate.
GB/T 714 adds the Z level to the end of the designation, for example Q550qEZ25. The test and acceptance follow GB/T 5313 and apply to plate 15 mm and thicker.
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
E chemistry already limits S to 0.010%, the Z15 sulfur cap. Z25 (S ≤0.007%) and Z35 (S ≤0.005%) still need a cleaner heat.
A Z level on Q550qE does not change strength or impact rules. It adds a sulfur cap and a short-transverse tensile test. Z options apply across the GB/T 714 bridge steel range.
Equivalent Material Grades
Annex B of GB/T 714-2025 lists foreign grades against each strength level. It is informative: it tells you which families are close, not that the plates are interchangeable.
| Standard | Grade(s) | Fit for Q550qE |
|---|---|---|
| EN 10025-6 | EN 10025-6 S550Q, EN 10025-6 S550QL, EN 10025-6 S550QL1 | Listed in Annex B |
| GB/T 16270 | GB/T 16270 Q550E | QT alternative, different toughness rules |
| GB/T 1591 | GB/T 1591 Q550ME | TMCP general structural |
Before substituting, compare three things line by line: minimum yield at the actual thickness, the impact test temperature and energy, and the weldability index. For Q550qE, the 120 J impact level and the Pcm/CEV caps are usually the hardest to match.
Q550qE Testing, UT and Certificate
A batch of Q550qE is one grade, one heat, one thickness, one rolling schedule and one heat-treatment condition, up to 60 t. Table 12 of GB/T 714-2025 sets the tests:
| Test | Frequency | Method |
|---|---|---|
| Heat analysis | 1 per heat | GB/T 20066; GB/T 4336 / GB/T 223 |
| Tensile | 1 per batch | GB/T 2975 / GB/T 228.1 |
| Bend 180° | 1 per batch (may be waived if guaranteed) | GB/T 232 |
| Charpy V at −40°C | 3 specimens per batch | GB/T 229 |
| Through-thickness (Z) | 3 specimens per batch, when ordered | GB/T 5313 |
| Ultrasonic | Every plate >20 mm, Class II or better | GB/T 2970 |
| Surface and dimensions | Every plate | Visual and gauges |
Impact retest: if a set fails, three more specimens are taken from the same batch. The average of all six must meet the requirement; two values may be below it, but only one below 70%. At −40°C, retest risk rises on heavy plate; we build a margin for retests into the delivery schedule.
Dimensions
Q550qE sizes we supply from mill and stock:
- Thickness: 6 mm – 100 mm under GB/T 714 tensile tables; most orders 10 – 60 mm
- Width: 1500 – 4000 mm, depending on mill and thickness
- Length: 6000 – 18000 mm; longer by enquiry
- Edge: mill edge or cut edge
- Weight: theoretical, 7.85 g/cm³
Deck plate, webs, flanges, diaphragms and stiffeners are cut to drawing. For U-ribs and rolled sections on the same bridge, see steel beam profiles and steel structural profiles.
Tolerances
Thickness, width, length, flatness and camber of Q550qE follow GB/T 709. The table shows Class B thickness limits for common sizes.
| Nominal thickness (mm) | Width ≤ 1500 mm | Width > 1500 – 2500 mm |
|---|---|---|
| > 8 – 15 | −0.30 / +0.80 | −0.30 / +1.00 |
| > 15 – 25 | −0.30 / +1.00 | −0.30 / +1.20 |
| > 25 – 40 | −0.30 / +1.10 | −0.30 / +1.30 |
| > 40 – 60 | −0.30 / +1.30 | −0.30 / +1.50 |
| > 60 – 100 | −0.30 / +1.50 | −0.30 / +1.80 |
| > 100 – 150 | −0.30 / +2.10 | −0.30 / +2.50 |
Bridge fabricators often ask for Class C (zero minus) on deck and flange plate so section properties are never under the design value. Wider plates follow the heavier GB/T 709 rows; we state them on the offer.
Q550qE Price Factors and How to Order
A Q550qE price per ton is a base price plus extras. The extras explain most gaps between quotes.
| Cost driver | Effect on price |
|---|---|
| Strength level Q550q | Higher levels need more alloy and tighter rolling control |
| Quality letter | Higher extra: −40°C testing, S ≤0.010%, more retest risk |
| Delivery route | TMCP / TMCP+T / QT; QT costs more than TMCP |
| Thickness | Over 60 mm and under 10 mm carry size extras |
| Z15 / Z25 / Z35 | Low-sulfur heat, Z test, UT; Z35 costs most |
| Width and length | Over 3000 mm wide or 15 m long needs mill confirmation |
| Quantity per size | Mill minimums per heat and size |
| Inspection and processing | 3.2 witness, profile cutting, blasting, priming quoted per item |
To get a firm quote in one round, send:
- Grade, edition and Z level, e.g. Q550qEZ25 to GB/T 714-2025
- Thickness × width × length and pieces or tonnes
- Delivery route and UT class if beyond Class II
- Certificate type and inspector
- Destination port and Incoterm
We quote plate price, extras and freight line by line. Need another letter? See Q550qD, Q550qF.
Applications
| Sector | Typical Q550qE components |
|---|---|
| Ultra-long-span bridges | Main truss chords and anchor zones |
| Cable-stayed bridges | Highly stressed box girder flanges |
| Steel pylons | Pylon wall plate |
| Railway bridges | Heavily loaded node plates |
| Weight-critical retrofits | Replacement members with limited depth |
The letter E suits bridges in north-east China, Inner Mongolia, Xinjiang, Russia, Kazakhstan, Canada and high-altitude sites, and for thick, restrained members anywhere.
It is the wrong plate for pressure equipment (pressure vessel steel plates), unpainted exposure (weathering steel plates) or ship hulls (shipbuilding steel plates).
Supply Capability and Global Delivery
SHH STEEL sources Q550qE from first-line bridge-plate mills, including drafters of GB/T 714-2025 such as Ansteel, Valin Xiangtan, Jiangyin Xingcheng, Wuyang, Shougang and Xinyu.
- Certificates: EN 10204 3.1 standard; 3.2 with third-party witness (SGS, BV, TÜV or owner’s inspector)
- Tests: tensile, −40°C Charpy, bend, Z test, UT, product analysis
- Processing: CNC plasma and flame cutting, bevelling, drilling, shot blasting and priming
- Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
- Marking: steel-stamped and paint-marked with grade, heat, size and mill, per GB/T 247
Buyers of Q550qE are usually bridge fabricators and EPC contractors working to Chinese drawings overseas. We ship worldwide.
Lead time: about 45–60 days from mill rolling; Z35, F letter or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Southeast Asia and 28–35 days to North Europe.
Why Choose SHH STEEL
SHH STEEL is a steel manufacturer and exporter and global steel mill sourcing partner. We buy Q550qE mill-direct, China origin, and check every certificate before shipment.
Before shipment we check four lines on every Q550qE certificate: yield and tensile for the actual thickness band, Charpy at −40°C, the CEV or Pcm for the delivery route, and UT results. If one fails, the plate does not ship as Q550qE.
For QT Q550qE, the CEV cap is 0.52% to 50 mm and 0.57% to 100 mm. Ask the fabricator to qualify procedures on the actual heat chemistry.
We also tell buyers when another grade fits better. Neighbouring levels are Q500qE and Q620qE. Browse more structural steel plates and high strength low alloy plates.
FAQ
-
What is Q550qE steel?
- Q550qE is bridge structural steel plate to GB/T 714-2025. It has 550 MPa minimum yield up to 50 mm, 660 MPa minimum tensile, 16% elongation and Charpy V-notch impact of 120 J at −40°C for 12–100 mm plate. It is delivered TMCP, TMCP + tempering, or quenched and tempered.
-
What is the difference between Q550qE and Q550qD?
- Strength and chemistry box are the same. Q550qE is Charpy tested at −40°C, Q550qD at −20°C, both needing 120 J for 12–100 mm plate. P/S caps are 0.020/0.010% for E and 0.025/0.015% for D. Choose by the lowest service or erection temperature.
-
What is the maximum thickness of Q550qE?
- GB/T 714-2025 covers bridge plate up to 150 mm, but tensile values for Q550q stop at 100 mm. Above that there is no table value, so Q550qE cannot be certified thicker than 100 mm without a special agreement.
-
What is the ASTM or EN equivalent of Q550qE?
- Close grades for Q550qE: EN 10025-6 S550Q, S550QL, S550QL1 (Annex B). These are close families, not drop-in substitutes; compare yield at thickness, impact temperature and energy, and the weldability index before substituting.
-
What is the batch size for GB/T 714 bridge plate testing?
- Up to 60 t of one grade, heat, thickness, rolling schedule and heat-treatment condition. Each batch gets one tensile test, one bend test and one set of three Charpy specimens; heat analysis is reported per heat.
-
What is the carbon equivalent of Q550qE?
- It depends on the route. For Q550qE up to 50 mm, GB/T 714-2025 sets Pcm ≤0.23% (TMCP) or CEV ≤0.52% (QT). CEV applies to normalized, QT and TMCP steel with C >0.12%; Pcm to TMCP steel with C ≤0.12%.
Conclusion
Q550qE to GB/T 714-2025 is bridge plate with 550 MPa minimum yield, 660 MPa minimum tensile and 120 J Charpy at −40°C for 12–100 mm plate.
It sits between Q500qE and Q620qE in the bridge range, with Q550qD and Q550qF as sister letters. We check every Q550qE order against GB/T 714-2025 before quoting, so the offer, the test plan and the certificate all match the drawing.
Every Q550qE plate from SHH STEEL ships with heat analysis, the weldability index, tensile and Charpy results on an EN 10204 3.1 or 3.2 certificate. Product analysis, Z15–Z35, extra UT and cut-to-size are options.
We ship from Shanghai to bridge builders worldwide. Browse the full GB/T 714 range or other high strength low alloy plates.
Send your enquiry with grade, edition, sizes and inspection needs, and we will answer within one working day. Contact SHH STEEL for Q550qE bridge steel plate.