GB/T 714 Q500qD bridge steel plate stacked at SHH STEEL warehouse

GB/T 714 Q500qD Bridge Steel Plate Supplier

GB/T 714 Q500qD is bridge structural steel plate with 500 MPa minimum yield, 630 MPa minimum tensile and Charpy V-notch impact of 120 J at −20°C for 12–100 mm plate. SHH STEEL supplies Q500qD mill-direct, TMCP / TMCP+T / QT, up to 130 mm, with Z15–Z35, UT and heat and product analysis.
Keywords
Q500qD, Q500qD steel plate, GB/T 714 Q500qD, Q500q-D, Q500q D, Q500qD bridge steel, Q500qDZ15, Q500qDZ25, Q500qDZ35, bridge steel plate, Q500qD supplier
Equivalent Grades:
EN 10025-4 S500M, S500ML / EN 10025-6 S500Q, S500QL, S500QL1 (Annex B) — Material Specification: GB/T 714-2025 (supersedes GB/T 714-2015) — Delivery: TMCP / TMCP+T / QT
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q500q Quality Grades
GB/T 714-2025 vs 2015
Q500qD vs ASTM A709 / EN 10025
TMCP vs Normalized vs QT
Welding and Fatigue
Z15 / Z25 / Z35
Equivalent Material Grades
Testing and Inspection
Dimensions
Tolerances
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 714 Q500qD Bridge Steel Plate?

Q500qD is bridge structural steel plate to GB/T 714. Q stands for yield, 500 is the minimum yield in MPa for plate up to 50 mm, q stands for qiao (bridge) and D is the quality grade: Charpy V-notch at −20°C on longitudinal specimens.

Q500q is the strongest grade that can still be bought TMCP or quenched and tempered at up to 130 mm, used on record-span railway and road-rail bridges. The Shanghai–Nantong Yangtze River Bridge, a road-rail cable-stayed bridge with a 1,092 m main span, was the first large project to use Q500qE. Q500q can be supplied TMCP (Pcm ≤0.23%) or QT (CEV ≤0.50%).

Q500qD offers 500 MPa yield with a −20°C Charpy, delivered TMCP or QT. It is used where Q460q would exceed 60 mm and the site does not need −40°C toughness.

Edition status: GB/T 714-2025 was published on 31 October 2025 and has applied since 1 May 2026. It fully replaces GB/T 714-2015. Orders signed under the 2015 edition can still be certified to it if the contract says so; new orders default to 2025.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q500qD cut to size with an EN 10204 3.1 or 3.2 certificate. Sister grades are listed under GB/T 714.

Material Specification

Specification element Requirement SHH STEEL compliance
Standard GB/T 714-2025 Q500qD Confirmed
Product Single-rolled plate ≤150 mm; hot-rolled strip and cut plate ≤25.4 mm Plate
Thickness with tensile values Up to 130 mm for Q500q Confirmed
Minimum yield ReL 500 MPa ≤50 mm; 480 MPa >50–100 mm Confirmed
Minimum tensile Rm 630 MPa ≤100 mm (no upper limit in the standard) Confirmed
Elongation A ≥ 18% Confirmed
Charpy V-notch −20°C, 120 J (12–100 mm), longitudinal Confirmed
Delivery condition TMCP, TMCP + tempering, or quenched and tempered (QT) As ordered
Weldability index Pcm (Table 7) for TMCP; CEV (Table 6) for QT Printed on MTC
Ultrasonic testing Plate >20 mm: GB/T 2970, Class II or better Every plate
Through-thickness Z15, Z25 or Z35 to GB/T 5313, when ordered As ordered
Dimensions GB/T 709 Confirmed
Certificate GB/T 247; EN 10204 3.1 or 3.2 As ordered

Grades often compared with Q500qD are EN 10025-6 S460Q and EN 10025-4 S460ML; the comparison below shows where they differ.

Chemical Composition: Heat Analysis and Product Analysis

Two analyses matter for Q500qD. The heat (ladle) analysis is taken during casting and printed on the certificate. The product analysis is taken from finished plate and judged with the wider GB/T 222 tolerances. Mixing the two is the most common reason for disputed rejections.

Table 1 below is the heat (ladle) analysis for Q500qD from GB/T 714-2025 Tables 1, 2, 3 and 4.

Element Q500qD TMCP (%) Q500q quenched and tempered (%)
C, max 0.11 0.11
Si, max 0.55 0.55
Mn 0.80 – 1.70 0.80 – 1.70
P, max 0.025 0.025
S, max 0.015 0.015
Nb 0.010 – 0.090 0.005 – 0.060
V 0.010 – 0.080 0.010 – 0.080
Ti 0.006 – 0.030 0.006 – 0.030
Als 0.010 – 0.045 0.010 – 0.045
Cr, max 0.80 ≤ 0.80
Ni, max 0.70 ≤ 0.70
Cu, max 0.30 ≤ 0.30
Mo, max 0.30 ≤ 0.30
N, max 0.0080 0.0080
B, max 0.0005 residual (≤0.0014 if C ≤0.10%) 0.0005–0.0030 may be added
H, max 0.0002 0.0002

Nb, V, Ti and Al may be added singly or together. Added singly, each must meet the range above; added together, at least one must reach its minimum and Nb + V + Ti ≤ 0.22%.

Table 2 is the product analysis: the limits a check analysis on finished plate is judged against. GB/T 714-2025 clause 7.1.3 calls up GB/T 222 for the permitted deviations.

Element Heat limit (%) Deviation, GB/T 222-2025 Table 1 Q500qD product analysis (%)
C ≤ 0.11 +0.02 ≤ 0.13
Si ≤ 0.55 +0.05 ≤ 0.60
Mn 0.80 – 1.70 ±0.06 0.74 – 1.76
P ≤ 0.025 +0.005 ≤ 0.030
S ≤ 0.015 +0.005 ≤ 0.020
V 0.010 – 0.080 +0.02 / −0.01 ≤ 0.100
Ti 0.006 – 0.030 +0.02 / −0.01 ≤ 0.050
Nb 0.010 – 0.090 ±0.005 (listed for 0.015–0.060%) Above 0.060%: agree in contract
Cr ≤ 0.80 +0.05 ≤ 0.85
Ni ≤ 0.70 +0.05 ≤ 0.75
Cu ≤ 0.30 +0.05 ≤ 0.35
Als 0.010 – 0.045 ±0.003 Lower limit −0.003 (Table 1 row is for Al ≥0.015%; confirm)
Mo ≤ 0.30 Not listed in Table 1 Agree in contract
N ≤ 0.0080 Listed only for 0.010–0.020% Agree in contract

How to read Table 2. Q500q TMCP heats are low-alloy steel, so Table 1 of GB/T 222 applies. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn falls in the 0.80–1.70% band, so ±0.06%. For one heat, an element may deviate in one direction only.

Mechanical Properties

Tensile values follow Table 9 of GB/T 714-2025 for Q500q. Tensile specimens are transverse; round specimens are used above 40 mm. Where yield is not distinct, Rp0.2 replaces ReL.

Nominal thickness ReL min (MPa) Rm min (MPa) A min
≤ 50 mm 500 630 18%
> 50 – 100 mm 480 630 18%
> 100 – 130 mm 450 560 18%

Impact values follow Table 10, on longitudinal specimens, average of three:

Letter / test temperature KV2 ≤12 mm KV2 >12 – 100 mm KV2 >100 – 150 mm
D / −20°C 80 J 120 J 47 J

One single value may fall below the required average, but not below 70% of it. Plate over 8 mm and under 12 mm is tested with 7.5 mm specimens (75% of the value); 6–8 mm plate with 5 mm specimens (50%). Plate under 6 mm is not impact tested.

180° bend test, transverse: mandrel D = 2a up to 16 mm and 3a above 16 mm; may be omitted when the mill guarantees it. Yield ratio is not mandatory. If the contract asks for it, Annex C recommends ReL/Rm ≤ 0.88 up to 12 mm and ≤ 0.86 above 12 mm for TMCP plate.

Q500qD / Q500qE / Q500qF: Which Quality Grade?

Q500qD is tested at −20°C. It suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C. D is the most specified letter on Chinese bridge drawings. It is tested at −20°C and the melt is tighter than C: P ≤0.025%, S ≤0.015%.

Grade Test temp. KV2 ≤12 mm KV2 12–100 mm KV2 >100 mm P / S max (%)
Q500qD −20°C 80 J 120 J 47 J 0.025 / 0.015
Q500qE −40°C 80 J 120 J 31 J 0.020 / 0.010
Q500qF −60°C By agreement 54 J — 0.015 / 0.006

Over-specifying the letter costs money; under-specifying it costs safety. Choose from the lowest service or erection temperature, then step up one letter for thick, restrained or fracture-critical members.

Q500qD: What Changed from GB/T 714-2015 to GB/T 714-2025

For Q500qD buyers the 2025 edition changes more than the year on the certificate. The points below come from the foreword of GB/T 714-2025 and its tables.

  • Yield values above 100 mm were added (450 MPa for >100–130 mm).
  • The Mn range for TMCP steel was revised: the minimum is now 0.80%, and the maximum may be raised to 2.00% by agreement.
  • CEV and Pcm limits were revised (Tables 6 and 7).
  • Tensile strength is now banded by thickness (e.g. lower minimum Rm above 100 mm) instead of one value.
  • Impact energy is set by thickness band (≤12 mm, 12–100 mm, >100 mm) in Table 10.
  • Yield ratio is no longer a clause value; it is agreed in the contract, with recommendations in informative Annex C.
  • Section products were removed; the standard now covers plate and strip only.
  • Delivery is TMCP, TMCP + tempering or QT; normalizing is kept only for Q345q/Q370q plate over 100 mm by agreement.

If a drawing cites 2015 and the plate is made to 2025, get the designer’s written acceptance; tensile strength above 100 mm and the yield-ratio basis differ.

Q500qD vs ASTM A709 and EN 10025: Which Grade Matches?

Can Q500qD replace a US or European bridge grade, or the other way round? Strength can match; toughness rules differ in kind, not only in number.

Property Q500qD EN 10025-6 S460Q EN 10025-4 S460ML EN 10025-6 S500Q
Min. yield (MPa) 500 (≤50 mm) 460 (≤50 mm) 460 (≤16 mm) 500 (≤50 mm)
Tensile (MPa) 630 min 550 – 720 540 – 720 590 – 770
Charpy 120 J at −20°C (12–100 mm) Q: −20°C, QL: −40°C, QL1: −60°C 27 J at −50°C Q / QL / QL1: −20 / −40 / −60°C
Weathering chemistry No No No No

ASTM A709 sets Charpy requirements by temperature zone (1, 2, 3) and by member type: non-fracture-critical (T) or fracture-critical (F). GB/T 714 sets one value per letter, so compare the A709 zone with the GB/T 714 test temperature, not grade with grade.

EN 10025-3/-4/-6 grades show yield at the thinnest band; their values fall with thickness. GB/T 714 keeps 500 MPa to 50 mm. EN tensile ranges have upper limits; GB/T 714 gives minimums only.

The 120 J requirement in GB/T 714 for 12–100 mm plate is several times the 27–40 J typical of general structural grades. That margin is the main reason bridge owners specify Q500qD rather than GB/T 1591 plate.

Q500qD Delivery Condition: TMCP vs Normalized vs Quenched and Tempered

GB/T 714-2025 clause 3.2 defines TMCP as rolling with the final deformation in a controlled temperature range, including accelerated cooling with or without tempering (self-tempering included) but excluding direct quenching and quench-and-temper. The delivery route must be stated on the certificate.

Route Available for Q500qD Weldability index Notes
TMCP Yes Pcm ≤0.23% (≤50 mm) C ≤0.11%; up to 130 mm
TMCP + tempering Yes Pcm Improves toughness uniformity
Quenched and tempered Yes CEV ≤0.50% (≤50 mm) C ≤0.11%; B 0.0005–0.0030% may be added
Normalized No — Not listed

Q500q is the first level where both TMCP and QT are listed. TMCP plate is leaner (Pcm-controlled); QT plate carries more alloy and is CEV-controlled, but its properties are usually more uniform through the thickness. D-letter plate is usually plain TMCP; tempering is added mainly for heavy plate or tight yield-ratio limits.

Ask for the route on the purchase order. It changes the weldability index, the welding procedure and, for heavy plate, the price of Q500qD.

Welding Q500qD and Fatigue in Bridge Girders

GB/T 714-2025 clause 7.1.2 uses CEV for normalized, QT and TMCP steel with C >0.12%, and Pcm for weathering steel and TMCP steel with C ≤0.12%, both from the heat analysis:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Index ≤50 mm >50–100 mm >100–130 mm
Pcm, TMCP (Table 7) ≤ 0.23 ≤ 0.25 ≤ 0.25
CEV, QT (Table 6) ≤ 0.50 ≤ 0.55 by agreement

Most bridge fabricators qualify Q500qD procedures on plate from the same mill and route as the production order. Changing mill or route mid-project usually means re-qualifying. At −20°C, most procedures qualified on TMCP plate pass HAZ impact without special measures; keep multi-wire SAW heat input inside the qualified band.

Typical consumables for Q500qD: E62-class consumables (AWS E9018M type).

Fatigue. Welded details govern fatigue life in a bridge, and their fatigue strength is set by detail category, not by yield strength. Higher-strength plate can carry higher stress ranges only if detailing improves too.

Fatigue design follows JTG D64 (highway) and TB 10091 (railway) in China, EN 1993-1-9 in Europe and AASHTO LRFD in the US; fabrication commonly follows TB 10212, JTG/T 3650 or AWS D1.5.

Q500qDZ15, Z25 and Z35: Through-Thickness Plate for Bridges

A Z grade is cheap insurance for heavily restrained joints. It caps sulfur and proves reduction of area in the thickness direction with a short-transverse tensile test.

GB/T 714 adds the Z level to the end of the designation, for example Q500qDZ25. The test and acceptance follow GB/T 5313 and apply to plate 15 mm and thicker.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

D chemistry allows S up to 0.015%. Z15 needs S ≤0.010% and Z25 needs ≤0.007%, so Z plate is still made from a dedicated low-sulfur heat.

Ask your designer which Q500qD plates are loaded through the thickness. Ordering Z35 on everything costs money and time without adding safety. Z options apply across the GB/T 714 bridge steel range.

Equivalent Material Grades

Annex B of GB/T 714-2025 lists foreign grades against each strength level. It is informative: it tells you which families are close, not that the plates are interchangeable.

Standard Grade(s) Fit for Q500qD
EN 10025-4 S500M, S500ML Listed in Annex B
EN 10025-6 EN 10025-6 S500Q, EN 10025-6 S500QL, EN 10025-6 S500QL1 Listed in Annex B
GB/T 16270 GB/T 16270 Q500D QT alternative, different toughness rules
GB/T 1591 GB/T 1591 Q500MD TMCP general structural
GB/T 714 (weathering twin) Q500qNHD Same strength, weathering chemistry

Before substituting, compare three things line by line: minimum yield at the actual thickness, the impact test temperature and energy, and the weldability index. For Q500qD, the 120 J impact level and the Pcm/CEV caps are usually the hardest to match.

Q500qD Testing, UT and Certificate

A batch of Q500qD is one grade, one heat, one thickness, one rolling schedule and one heat-treatment condition, up to 60 t. Table 12 of GB/T 714-2025 sets the tests:

Test Frequency Method
Heat analysis 1 per heat GB/T 20066; GB/T 4336 / GB/T 223
Tensile 1 per batch GB/T 2975 / GB/T 228.1
Bend 180° 1 per batch (may be waived if guaranteed) GB/T 232
Charpy V at −20°C 3 specimens per batch GB/T 229
Through-thickness (Z) 3 specimens per batch, when ordered GB/T 5313
Ultrasonic Every plate >20 mm, Class II or better GB/T 2970
Surface and dimensions Every plate Visual and gauges

Impact retest: if a set fails, three more specimens are taken from the same batch. The average of all six must meet the requirement; two values may be below it, but only one below 70%. At −20°C the 120 J level is comfortable for well-made TMCP plate, but we still check each batch value, not just the average.

Dimensions

Q500qD plate sizes we regularly ship:

  • Thickness: 6 mm – 130 mm under GB/T 714 tensile tables; most orders 10 – 80 mm
  • Width: 1500 – 4000 mm, depending on mill and thickness
  • Length: 6000 – 18000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, 7.85 g/cm³

Deck plate, webs, flanges, diaphragms and stiffeners are cut to drawing. For U-ribs and rolled sections on the same bridge, see steel beam profiles and steel structural profiles.

Tolerances

GB/T 714-2025 clause 7.6 sends dimensions and shape to GB/T 709. Thickness tolerance is Class B by default: −0.30 mm fixed, plus side by thickness and width.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Bridge fabricators often ask for Class C (zero minus) on deck and flange plate so section properties are never under the design value. Wider plates follow the heavier GB/T 709 rows; we state them on the offer.

Q500qD Price Factors and How to Order

Two Q500qD quotes can differ a lot and both be fair. Base prices are similar; extras are where mills part.

Cost driver Effect on price
Strength level Q500q Higher levels need more alloy and tighter rolling control
Quality letter Small extra for −20°C testing and cleaner melt
Delivery route TMCP / TMCP+T / QT; QT costs more than TMCP
Thickness Over 60 mm and under 10 mm carry size extras
Z15 / Z25 / Z35 Low-sulfur heat, Z test, UT; Z35 costs most
Width and length Over 3000 mm wide or 15 m long needs mill confirmation
Quantity per size Mill minimums per heat and size
Inspection and processing 3.2 witness, profile cutting, blasting, priming quoted per item

To get a firm quote in one round, send:

  • Grade, edition and Z level, e.g. Q500qDZ25 to GB/T 714-2025
  • Thickness × width × length and pieces or tonnes
  • Delivery route and UT class if beyond Class II
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line. Need another letter? See Q500qE, Q500qF.

Applications

Sector Typical Q500qD components
Road-rail cable-stayed bridges Main truss chords and node plates
Suspension bridges Stiffening girder chords
Long-span arches Arch rib flanges
Steel pylons Pylon shell plate and anchor zones
Heavy railway bridges Members where Q460q exceeds 60 mm

The letter D suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C.

It is the wrong plate for pressure equipment (pressure vessel steel plates), unpainted exposure (weathering steel plates) or ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q500qD from first-line bridge-plate mills, including drafters of GB/T 714-2025 such as Ansteel, Valin Xiangtan, Jiangyin Xingcheng, Wuyang, Shougang and Xinyu.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness (SGS, BV, TÜV or owner’s inspector)
  • Tests: tensile, −20°C Charpy, bend, Z test, UT, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blasting and priming
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill, per GB/T 247

Buyers of Q500qD are usually bridge fabricators and EPC contractors working to Chinese drawings overseas. We ship worldwide.

Lead time: about 45–60 days from mill rolling; Z35, F letter or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Southeast Asia and 28–35 days to North Europe.

Why Choose SHH STEEL

SHH STEEL is mill-direct: steel manufacturer and exporter and global steel mill sourcing partner, China origin. Every Q500qD plate we ship carries the original mill heat number.

Before shipment we check four lines on every Q500qD certificate: yield and tensile for the actual thickness band, Charpy at −20°C, the CEV or Pcm for the delivery route, and UT results. If one fails, the plate does not ship as Q500qD.

Choose the route before ordering. TMCP Q500qD is judged by Pcm (≤0.23% to 50 mm); QT Q500qD by CEV (≤0.50% to 50 mm). The welding procedures differ.

We also tell buyers when another grade fits better. Neighbouring levels are Q460qD and Q550qD. The weathering counterpart is Q500qNHD. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q500qD steel?
Q500qD is bridge structural steel plate to GB/T 714-2025. It has 500 MPa minimum yield up to 50 mm, 630 MPa minimum tensile, 18% elongation and Charpy V-notch impact of 120 J at −20°C for 12–100 mm plate. It is delivered TMCP, TMCP + tempering, or quenched and tempered.
What is the difference between Q500qD and Q500qE?
Strength and chemistry box are the same. Q500qD is Charpy tested at −20°C, Q500qE at −40°C, both needing 120 J for 12–100 mm plate. P/S caps are 0.025/0.015% for D and 0.020/0.010% for E. Choose by the lowest service or erection temperature.
Is Q500q bridge steel TMCP or quenched and tempered?
Both are allowed by GB/T 714-2025. TMCP Q500q has C ≤0.11% and is judged by Pcm (≤0.23% to 50 mm); QT Q500q is judged by CEV (≤0.50% to 50 mm, ≤0.55% to 100 mm). The route must be stated on the order and the certificate.
What is the ASTM or EN equivalent of Q500qD?
Close grades for Q500qD: EN 10025-4 S500M, S500ML / EN 10025-6 S500Q, S500QL, S500QL1 (Annex B). These are close families, not drop-in substitutes; compare yield at thickness, impact temperature and energy, and the weldability index before substituting.
Can GB/T 714 bridge plate be normalized?
Only in one case. GB/T 714-2025 clause 6.2 requires TMCP, TMCP + tempering or quenched and tempered delivery, but Q345q and Q370q plate over 100 mm and up to 150 mm may be normalized by agreement.
Is Q500qD weldable?
Yes. GB/T 714-2025 caps the weldability index for Q500qD up to 50 mm at Pcm ≤0.23% (TMCP) or CEV ≤0.50% (QT). Preheat depends on actual chemistry, thickness and restraint, and is fixed by the qualified welding procedure.

Conclusion

Q500qD to GB/T 714-2025 is bridge plate with 500 MPa minimum yield, 630 MPa minimum tensile and 120 J Charpy at −20°C for 12–100 mm plate.

It sits between Q460qD and Q550qD in the bridge range, with Q500qE and Q500qF as sister letters. The most common ordering mistake with Q500qD is leaving the Z level, UT class or impact position off the order; add them at enquiry stage, not after rolling.

SHH STEEL ships Q500qD with heat analysis, weldability index and mechanical results on every certificate. Third-party inspection, product analysis and Z testing are added on request.

We ship from Shanghai to bridge builders worldwide. Browse the full GB/T 714 range or other high strength low alloy plates.

Send the edition, quality letter, Z level and size list; we confirm mill, delivery route, lead time and price in one reply. Contact SHH STEEL for a mill-direct quotation on Q500qD bridge steel plate.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X