GB/T 714 Q420qE bridge steel plate stacked at SHH STEEL warehouse

GB/T 714 Q420qE Bridge Steel Plate Supplier

GB/T 714 Q420qE is bridge structural steel plate with 420 MPa minimum yield, 540 MPa minimum tensile and Charpy V-notch impact of 120 J at −40°C for 12–100 mm plate. SHH STEEL supplies Q420qE mill-direct, TMCP / TMCP+T, up to 130 mm, with Z15–Z35, UT and heat and product analysis.
Keywords
Q420qE, Q420qE steel plate, GB/T 714 Q420qE, Q420q-E, Q420q E, Q420qE bridge steel, Q420qEZ15, Q420qEZ25, Q420qEZ35, bridge steel plate, Q420qE supplier
Equivalent Grades:
EN 10025-4 S420M, S420ML (Annex B) / ASTM A572 Gr.60 (strength only) — Material Specification: GB/T 714-2025 (supersedes GB/T 714-2015) — Delivery: TMCP / TMCP+T
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q420q Quality Grades
GB/T 714-2025 vs 2015
Q420qE vs ASTM A709 / EN 10025
TMCP vs Normalized vs QT
Welding and Fatigue
Z15 / Z25 / Z35
Equivalent Material Grades
Testing and Inspection
Dimensions
Tolerances
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 714 Q420qE Bridge Steel Plate?

Q420qE is bridge structural steel plate to GB/T 714. Q stands for yield, 420 is the minimum yield in MPa for plate up to 50 mm, q stands for qiao (bridge) and E is the quality grade: Charpy V-notch at −40°C on longitudinal specimens.

Q420q is the first of the lean-carbon high-strength bridge grades (C ≤0.11%), used for main trusses and box girders on long-span bridges. Q420q moves to a C ≤0.11% TMCP chemistry and is judged by Pcm (≤0.22%) instead of CEV. China’s first large Q420qE application was the Nanjing Dashengguan Yangtze River Bridge, a six-track high-speed railway arch bridge.

Q420qE made its name on the Nanjing Dashengguan Yangtze River Bridge, the first large Chinese bridge to use it. Today it is a standard choice for main trusses on long-span railway bridges: 420 MPa yield, 120 J at −40°C from 12 to 100 mm.

Which edition applies? GB/T 714-2025, in force since 1 May 2026, replaces GB/T 714-2015 in full. Drawings issued before 2026 often still cite 2015; we can certify to either, but the certificate will name one edition, not both.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q420qE cut to size with an EN 10204 3.1 or 3.2 certificate. Sister grades are listed under GB/T 714.

Material Specification

Specification element Requirement SHH STEEL compliance
Standard GB/T 714-2025 Q420qE Confirmed
Product Single-rolled plate ≤150 mm; hot-rolled strip and cut plate ≤25.4 mm Plate
Thickness with tensile values Up to 130 mm for Q420q Confirmed
Minimum yield ReL 420 MPa ≤50 mm; 410 MPa >50–100 mm Confirmed
Minimum tensile Rm 540 MPa ≤100 mm (no upper limit in the standard) Confirmed
Elongation A ≥ 19% Confirmed
Charpy V-notch −40°C, 120 J (12–100 mm), longitudinal Confirmed
Delivery condition TMCP or TMCP + tempering As ordered
Weldability index Pcm (Table 7) Printed on MTC
Ultrasonic testing Plate >20 mm: GB/T 2970, Class II or better Every plate
Through-thickness Z15, Z25 or Z35 to GB/T 5313, when ordered As ordered
Dimensions GB/T 709 Confirmed
Certificate GB/T 247; EN 10204 3.1 or 3.2 As ordered

Grades often compared with Q420qE are EN 10025-4 S420M, EN 10025-4 S420ML and ASTM A572 Gr.60; the comparison below shows where they differ.

Chemical Composition: Heat Analysis and Product Analysis

For Q420qE we report heat analysis on every certificate and add a product analysis when the buyer asks for it. The two use different limits: heat values follow GB/T 714, product values add the GB/T 222 deviations.

Table 1 below is the heat (ladle) analysis for Q420qE from GB/T 714-2025 Tables 1, 3.

Element Q420qE TMCP (%)
C, max 0.11
Si, max 0.55
Mn 0.80 – 1.70
P, max 0.020
S, max 0.010
Nb 0.010 – 0.090
V 0.010 – 0.080
Ti 0.006 – 0.030
Als 0.010 – 0.045
Cr, max 0.50
Ni, max 0.30
Cu, max 0.30
Mo, max 0.20
N, max 0.0080
B, max 0.0005 residual (≤0.0014 if C ≤0.10%)
H, max 0.0002

Nb, V, Ti and Al may be added singly or together. Added singly, each must meet the range above; added together, at least one must reach its minimum and Nb + V + Ti ≤ 0.22%.

Table 2 is the product analysis: the limits a check analysis on finished plate is judged against. GB/T 714-2025 clause 7.1.3 calls up GB/T 222 for the permitted deviations.

Element Heat limit (%) Deviation, GB/T 222-2025 Table 1 Q420qE product analysis (%)
C ≤ 0.11 +0.02 ≤ 0.13
Si ≤ 0.55 +0.05 ≤ 0.60
Mn 0.80 – 1.70 ±0.06 0.74 – 1.76
P ≤ 0.020 +0.005 ≤ 0.025
S ≤ 0.010 +0.005 ≤ 0.015
V 0.010 – 0.080 +0.02 / −0.01 ≤ 0.100
Ti 0.006 – 0.030 +0.02 / −0.01 ≤ 0.050
Nb 0.010 – 0.090 ±0.005 (listed for 0.015–0.060%) Above 0.060%: agree in contract
Cr ≤ 0.50 +0.05 ≤ 0.55
Ni ≤ 0.30 +0.05 ≤ 0.35
Cu ≤ 0.30 +0.05 ≤ 0.35
Als 0.010 – 0.045 ±0.003 Lower limit −0.003 (Table 1 row is for Al ≥0.015%; confirm)
Mo ≤ 0.20 Not listed in Table 1 Agree in contract
N ≤ 0.0080 Listed only for 0.010–0.020% Agree in contract

How to read Table 2. Q420q TMCP heats are low-alloy steel, so Table 1 of GB/T 222 applies. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn falls in the 0.80–1.70% band, so ±0.06%. For one heat, an element may deviate in one direction only.

Mechanical Properties

Tensile values follow Table 9 of GB/T 714-2025 for Q420q. Tensile specimens are transverse; round specimens are used above 40 mm. Where yield is not distinct, Rp0.2 replaces ReL.

Nominal thickness ReL min (MPa) Rm min (MPa) A min
≤ 50 mm 420 540 19%
> 50 – 100 mm 410 540 19%
> 100 – 130 mm 365 460 19%

Impact values follow Table 10, on longitudinal specimens, average of three:

Letter / test temperature KV2 ≤12 mm KV2 >12 – 100 mm KV2 >100 – 150 mm
E / −40°C 80 J 120 J 31 J

One single value may fall below the required average, but not below 70% of it. Plate over 8 mm and under 12 mm is tested with 7.5 mm specimens (75% of the value); 6–8 mm plate with 5 mm specimens (50%). Plate under 6 mm is not impact tested.

180° bend test, transverse: mandrel D = 2a up to 16 mm and 3a above 16 mm; may be omitted when the mill guarantees it. Yield ratio is not mandatory. If the contract asks for it, Annex C recommends ReL/Rm ≤ 0.88 up to 12 mm and ≤ 0.86 above 12 mm for TMCP plate.

Q420qD / Q420qE / Q420qF: Which Quality Grade?

Q420qE is tested at −40°C. It suits bridges in north-east China, Inner Mongolia, Xinjiang, Russia, Kazakhstan, Canada and high-altitude sites, and for thick, restrained members anywhere. E is tested at −40°C, with P ≤0.020% and S ≤0.010%. Many long-span bridges specify E even in mild climates, because thick plate and heavy welding raise the risk of brittle fracture.

Grade Test temp. KV2 ≤12 mm KV2 12–100 mm KV2 >100 mm P / S max (%)
Q420qD −20°C 80 J 120 J 47 J 0.025 / 0.015
Q420qE −40°C 80 J 120 J 31 J 0.020 / 0.010
Q420qF −60°C By agreement 47 J — 0.015 / 0.006

Over-specifying the letter costs money; under-specifying it costs safety. Choose from the lowest service or erection temperature, then step up one letter for thick, restrained or fracture-critical members.

Q420qE: What Changed from GB/T 714-2015 to GB/T 714-2025

For Q420qE buyers the 2025 edition changes more than the year on the certificate. The points below come from the foreword of GB/T 714-2025 and its tables.

  • Yield values above 100 mm were added (365 MPa for >100–130 mm).
  • The Mn range for TMCP steel was revised: the minimum is now 0.80%, and the maximum may be raised to 2.00% by agreement.
  • CEV and Pcm limits were revised (Tables 6 and 7).
  • Tensile strength is now banded by thickness (e.g. lower minimum Rm above 100 mm) instead of one value.
  • Impact energy is set by thickness band (≤12 mm, 12–100 mm, >100 mm) in Table 10.
  • Yield ratio is no longer a clause value; it is agreed in the contract, with recommendations in informative Annex C.
  • Section products were removed; the standard now covers plate and strip only.
  • Delivery is TMCP, TMCP + tempering or QT; normalizing is kept only for Q345q/Q370q plate over 100 mm by agreement.

If a drawing cites 2015 and the plate is made to 2025, get the designer’s written acceptance; tensile strength above 100 mm and the yield-ratio basis differ.

Q420qE vs ASTM A709 and EN 10025: Which Grade Matches?

Can Q420qE replace a US or European bridge grade, or the other way round? Strength can match; toughness rules differ in kind, not only in number.

Property Q420qE EN 10025-4 S420M EN 10025-4 S420ML ASTM A572 Gr.60
Min. yield (MPa) 420 (≤50 mm) 420 (≤16 mm) 420 (≤16 mm) 415
Tensile (MPa) 540 min 520 – 680 520 – 680 520 min
Charpy 120 J at −40°C (12–100 mm) 40 J at −20°C 27 J at −50°C Supplementary only
Weathering chemistry No No No No

ASTM A709 sets Charpy requirements by temperature zone (1, 2, 3) and by member type: non-fracture-critical (T) or fracture-critical (F). GB/T 714 sets one value per letter, so compare the A709 zone with the GB/T 714 test temperature, not grade with grade.

EN 10025-3/-4/-6 grades show yield at the thinnest band; their values fall with thickness. GB/T 714 keeps 420 MPa to 50 mm. EN tensile ranges have upper limits; GB/T 714 gives minimums only.

The 120 J requirement in GB/T 714 for 12–100 mm plate is several times the 27–40 J typical of general structural grades. That margin is the main reason bridge owners specify Q420qE rather than GB/T 1591 plate.

Q420qE Delivery Condition: TMCP vs Normalized vs Quenched and Tempered

GB/T 714-2025 clause 3.2 defines TMCP as rolling with the final deformation in a controlled temperature range, including accelerated cooling with or without tempering (self-tempering included) but excluding direct quenching and quench-and-temper. The delivery route must be stated on the certificate.

Route Available for Q420qE Weldability index Notes
TMCP Yes, standard Pcm (C ≤0.11%) Up to 130 mm
TMCP + tempering Yes Same as TMCP Common on thick or E/F plate
Normalized No — Dropped in 2025 for this level
Quenched and tempered Not listed — Use GB/T 16270 if QT is required

Q420q is a TMCP grade with C ≤0.11%, so weldability is judged by Pcm. TMCP + tempering is often used on E and F plate to improve toughness scatter. For E-letter plate over about 50 mm, many mills add tempering after TMCP to reduce toughness scatter through the thickness.

Ask for the route on the purchase order. It changes the weldability index, the welding procedure and, for heavy plate, the price of Q420qE.

Welding Q420qE and Fatigue in Bridge Girders

GB/T 714-2025 clause 7.1.2 uses CEV for normalized, QT and TMCP steel with C >0.12%, and Pcm for weathering steel and TMCP steel with C ≤0.12%, both from the heat analysis:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Index ≤50 mm >50–100 mm >100–130 mm
Pcm, TMCP (Table 7) ≤ 0.22 ≤ 0.22 ≤ 0.22

For Q420qE, ask the fabricator which index the WPS was qualified on. Where the WPS uses CEV and the standard uses Pcm, we print both on the certificate. At −40°C, HAZ toughness often becomes the limit. Fabricators usually cap heat input and qualify the procedure at −40°C on plate from the same route.

Typical consumables for Q420qE: E55-class low-hydrogen consumables (AWS E8018 type).

Fatigue. Welded details govern fatigue life in a bridge, and their fatigue strength is set by detail category, not by yield strength. Higher-strength plate can carry higher stress ranges only if detailing improves too.

Fatigue design follows JTG D64 (highway) and TB 10091 (railway) in China, EN 1993-1-9 in Europe and AASHTO LRFD in the US; fabrication commonly follows TB 10212, JTG/T 3650 or AWS D1.5.

Q420qEZ15, Z25 and Z35: Through-Thickness Plate for Bridges

When a bridge drawing marks a plate Z25, the mill must supply a low-sulfur heat and prove reduction of area through the thickness on every batch.

GB/T 714 adds the Z level to the end of the designation, for example Q420qEZ25. The test and acceptance follow GB/T 5313 and apply to plate 15 mm and thicker.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

E chemistry already limits S to 0.010%, the Z15 sulfur cap. Z25 (S ≤0.007%) and Z35 (S ≤0.005%) still need a cleaner heat.

A Z level on Q420qE does not change strength or impact rules. It adds a sulfur cap and a short-transverse tensile test. Z options apply across the GB/T 714 bridge steel range.

Equivalent Material Grades

Annex B of GB/T 714-2025 lists foreign grades against each strength level. It is informative: it tells you which families are close, not that the plates are interchangeable.

Standard Grade(s) Fit for Q420qE
EN 10025-4 EN 10025-4 S420M, EN 10025-4 S420ML Listed in Annex B
EN 10025-3 EN 10025-3 S420N, EN 10025-3 S420NL Normalized alternative
ASTM A572 ASTM A572 Gr.60 Strength only, not a bridge grade
GB/T 1591 GB/T 1591 Q420ME General structural
GB/T 714 (weathering twin) Q420qNHE Same strength, weathering chemistry

Before substituting, compare three things line by line: minimum yield at the actual thickness, the impact test temperature and energy, and the weldability index. For Q420qE, the 120 J impact level and the Pcm/CEV caps are usually the hardest to match.

Q420qE Testing, UT and Certificate

A batch of Q420qE is one grade, one heat, one thickness, one rolling schedule and one heat-treatment condition, up to 60 t. Table 12 of GB/T 714-2025 sets the tests:

Test Frequency Method
Heat analysis 1 per heat GB/T 20066; GB/T 4336 / GB/T 223
Tensile 1 per batch GB/T 2975 / GB/T 228.1
Bend 180° 1 per batch (may be waived if guaranteed) GB/T 232
Charpy V at −40°C 3 specimens per batch GB/T 229
Through-thickness (Z) 3 specimens per batch, when ordered GB/T 5313
Ultrasonic Every plate >20 mm, Class II or better GB/T 2970
Surface and dimensions Every plate Visual and gauges

Impact retest: if a set fails, three more specimens are taken from the same batch. The average of all six must meet the requirement; two values may be below it, but only one below 70%. At −40°C, retest risk rises on heavy plate; we build a margin for retests into the delivery schedule.

Dimensions

Usual Q420qE supply range from SHH STEEL:

  • Thickness: 6 mm – 130 mm under GB/T 714 tensile tables; most orders 10 – 80 mm
  • Width: 1500 – 4000 mm, depending on mill and thickness
  • Length: 6000 – 18000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, 7.85 g/cm³

Deck plate, webs, flanges, diaphragms and stiffeners are cut to drawing. For U-ribs and rolled sections on the same bridge, see steel beam profiles and steel structural profiles.

Tolerances

GB/T 709 governs Q420qE thickness, width, length and flatness. Under Class B, plate may be up to 0.30 mm thin; the plus side grows with thickness and width.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Bridge fabricators often ask for Class C (zero minus) on deck and flange plate so section properties are never under the design value. Wider plates follow the heavier GB/T 709 rows; we state them on the offer.

Q420qE Price Factors and How to Order

When you compare Q420qE offers, compare extras line by line. These are the items that move the price.

Cost driver Effect on price
Strength level Q420q Higher levels need more alloy and tighter rolling control
Quality letter Higher extra: −40°C testing, S ≤0.010%, more retest risk
Delivery route TMCP / TMCP+T
Thickness Over 60 mm and under 10 mm carry size extras
Z15 / Z25 / Z35 Low-sulfur heat, Z test, UT; Z35 costs most
Width and length Over 3000 mm wide or 15 m long needs mill confirmation
Quantity per size Mill minimums per heat and size
Inspection and processing 3.2 witness, profile cutting, blasting, priming quoted per item

To get a firm quote in one round, send:

  • Grade, edition and Z level, e.g. Q420qEZ25 to GB/T 714-2025
  • Thickness × width × length and pieces or tonnes
  • Delivery route and UT class if beyond Class II
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line. Need another letter? See Q420qD, Q420qF.

Applications

Sector Typical Q420qE components
Long-span railway bridges Main truss chords and node plates
Cable-stayed bridges Steel box girders, anchor boxes
Suspension bridges Stiffening girders
Combined road-rail bridges Truss members carrying heavy rail load
Arch bridges Arch ribs and hangers’ anchorages

The letter E suits bridges in north-east China, Inner Mongolia, Xinjiang, Russia, Kazakhstan, Canada and high-altitude sites, and for thick, restrained members anywhere.

It is the wrong plate for pressure equipment (pressure vessel steel plates), unpainted exposure (weathering steel plates) or ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q420qE from first-line bridge-plate mills, including drafters of GB/T 714-2025 such as Ansteel, Valin Xiangtan, Jiangyin Xingcheng, Wuyang, Shougang and Xinyu.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness (SGS, BV, TÜV or owner’s inspector)
  • Tests: tensile, −40°C Charpy, bend, Z test, UT, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blasting and priming
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill, per GB/T 247

We ship Q420qE to fabricators in Asia, Africa, the Middle East, Europe and the Americas, by break-bulk or container.

Lead time: about 45–60 days from mill rolling; Z35, F letter or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Southeast Asia and 28–35 days to North Europe.

Why Choose SHH STEEL

SHH STEEL has supplied bridge plate as a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. Q420qE is ordered from mills that roll bridge steel every month.

Before shipment we check four lines on every Q420qE certificate: yield and tensile for the actual thickness band, Charpy at −40°C, the CEV or Pcm for the delivery route, and UT results. If one fails, the plate does not ship as Q420qE.

For truss node plates in Q420qE, order Z25 and a GB/T 2970 class beyond the Class II minimum if the joint design is highly restrained.

We also tell buyers when another grade fits better. Neighbouring levels are Q390q and Q460qE. The weathering counterpart is Q420qNHE. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q420qE steel?
Q420qE is bridge structural steel plate to GB/T 714-2025. It has 420 MPa minimum yield up to 50 mm, 540 MPa minimum tensile, 19% elongation and Charpy V-notch impact of 120 J at −40°C for 12–100 mm plate. It is delivered TMCP or TMCP + tempering.
What is the difference between Q420qE and Q420qD?
Strength and chemistry box are the same. Q420qE is Charpy tested at −40°C, Q420qD at −20°C, both needing 120 J for 12–100 mm plate. P/S caps are 0.020/0.010% for E and 0.025/0.015% for D. Choose by the lowest service or erection temperature.
What is the yield strength of Q420qE?
Q420qE has a minimum lower yield strength of 420 MPa up to 50 mm and 410 MPa from 50 to 100 mm, and 365 MPa from 100 to 130 mm (GB/T 714-2025 Table 9). Minimum tensile is 540 MPa up to 100 mm. There is no upper tensile limit in the standard.
What is the ASTM or EN equivalent of Q420qE?
Close grades for Q420qE: EN 10025-4 S420M, S420ML (Annex B) / ASTM A572 Gr.60 (strength only). These are close families, not drop-in substitutes; compare yield at thickness, impact temperature and energy, and the weldability index before substituting.
Does Q420qE have a yield ratio requirement?
Not a mandatory one. GB/T 714-2025 clause 7.7 lets the buyer set a yield ratio in the contract. Annex C recommends ReL/Rm ≤0.88 up to 12 mm and ≤0.86 above 12 mm for TMCP plate at the Q420q level.
What is the carbon equivalent of Q420qE?
It depends on the route. For Q420qE up to 50 mm, GB/T 714-2025 sets Pcm ≤0.22%. CEV applies to normalized, QT and TMCP steel with C >0.12%; Pcm to TMCP steel with C ≤0.12%.

Conclusion

Q420qE to GB/T 714-2025 is bridge plate with 420 MPa minimum yield, 540 MPa minimum tensile and 120 J Charpy at −40°C for 12–100 mm plate.

It sits between Q390q and Q460qE in the bridge range, with Q420qD and Q420qF as sister letters. We check every Q420qE order against GB/T 714-2025 before quoting, so the offer, the test plan and the certificate all match the drawing.

SHH STEEL supplies Q420qE with heat analysis, Pcm or CEV, tensile and Charpy results on an EN 10204 3.1 or 3.2 certificate, and adds product analysis to GB/T 222 when you need it.

We ship from Shanghai to bridge builders worldwide. Browse the full GB/T 714 range or other high strength low alloy plates.

Tell us the sizes, tonnage and any Z, UT or inspection needs. We check the request against GB/T 714 first, then confirm mill, route, lead time and price. Contact SHH STEEL today for Q420qE bridge steel plate.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X