ASME SA312 TP310S Stainless Steel Pipe | ASME SA312 Stainless Steel - SHH STEEL

ASME SA312 TP310S Stainless Steel Pipe | SA 312/SA 312M

ASME SA312 TP310S (UNS S31008) stainless steel pipe under SA-312/SA-312M (ASTM A312/A312M): seamless (SML), welded (WLD) and heavily cold-worked (HCW); Cr 24.0–26.0%, Ni 19.0–22.0%, C ≤0.08%, Si ≤1.00%, Mo ≤0.75%; Table 4 minima 75/30 ksi; solution annealed. SHH STEEL supplies with EN 10204 3.1 MTCs.
Grade
TP310S / UNS S31008
Standard
ASME SA312 / SA 312M (ASTM A312 / A312M)
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA312 TP310S Stainless Steel Pipe

ASME SA-312/SA-312M covers seamless, welded, and heavily cold-worked austenitic stainless steel pipe intended for high-temperature and general corrosive service. Grade TP310S is listed in Table 1 as UNS S31008. Commercially the same product may be called SA312 TP310S pipe, ASTM A312 TP310S pipe, A312 Grade TP310S, 310S, or 25-20 stainless steel pipe when the purchase order clearly references SA-312 or A312. For pressure piping and code work, cite the full grade designation, the UNS number, and the edition of the standard on the purchase order and on the mill test certificate—do not rely on a bare “310S” or “25-20” market label.

TP310S is the workhorse low-carbon member of the 25Cr–20Ni (310) family. Table 1 locks carbon at ≤0.08%, sets chromium at 24.0–26.0% and nickel at 19.0–22.0%, lists silicon ≤1.00%, and keeps molybdenum as a residual ceiling of ≤0.75% (not an intentional alloying addition for chloride service). That chemistry supports the Table 4 tensile floor of 75 ksi [515 MPa] min / 30 ksi [205 MPa] min yield while delivering stronger high-temperature oxidation resistance than the 309 family. It is not an H grade: carbon is a maximum only (no 0.04% floor), Table 2 uses the default solution-annealing temperature of 1900 °F [1040 °C] because S31008 is not individually listed, Table 5 does not mandate grain-size control, and clause 6.2 reheat language does not apply. Table 6 shows an ellipsis (“…”) for the AWS filler class of TP310S / S31008, so filler selection is by agreement on the WPS—not asserted here as a Table 6 mandate.

SHH STEEL can supply ASME SA312 TP310S stainless steel pipe to the edition named on the enquiry, including seamless (SML), welded (WLD), and heavily cold-worked (HCW) routes; ASME B36.19 schedules and special OD/wall by agreement; EN 10204 3.1 mill test certificates; and dual SA-312/A312 marking when the heat analysis, heat treatment, mechanical tests, and marking satisfy both editions named on the purchase order. Confirm NPS, wall or schedule, finish, length practice, and any product-analysis or supplementary tests on enquiry.

Common commercial names and how they map to the ordered product are listed below—use the full SA-312/A312 designation on the purchase order rather than market shorthand alone.

  • ASME SA312 TP310S / SA-312 Grade TP310S — preferred marking language for ASME-code and dual-marked pipe
  • ASTM A312 TP310S — same grade tables for chemistry and tensile when the ASTM edition is referenced
  • UNS S31008 — unified numbering system identity used on MTCs, stencils, and Section II Part D cross-references
  • 310S / 25-20 stainless steel pipe — market shorthand; confirm C ≤0.08%, Cr 24–26%, Ni 19–22%, Si ≤1.00%, and Mo ≤0.75% on the order

TP310S is not a drop-in for ASME SA312 UNS S31002 Stainless Steel Pipe, ASME SA312 TP310H Stainless Steel Pipe, ASME SA312 TP310Cb Stainless Steel Pipe, or ASME SA312 TP309S Stainless Steel Pipe on a shared “310” or “25-20” market label—each has its own Table 1 row. Versus UNS S31002, TP310S allows C ≤0.08% (vs ≤0.015%), Si ≤1.00% (vs ≤0.15%), Mo ≤0.75% (vs ≤0.10%), and carries a 75 ksi tensile floor instead of 73 ksi—commodity 310S heats will never meet S31002. Versus TP310H, TP310S has no carbon floor, no Table 5 grain-size rule, and no clause 6.2 reheat mandate; dual 310S/310H marking is possible only when carbon also meets the 0.04–0.10% H band and grain size is controlled. Versus TP310Cb, TP310S has no niobium stabilization. Versus TP309S (Cr 22–24, Ni 12–15), TP310S sits one step higher in alloy content for hotter oxidation service. Hub: ASME SA 312/SA 312M.

Manufacturing Types (SML / WLD / HCW)

ASME SA-312 defines three manufacturing routes that may be marked on finished TP310S pipe. Selecting the route is a purchase-order decision driven by design code, size range, wall thickness, and inspection preference. It does not change the Table 1 chemistry of UNS S31008—melting must still meet C ≤0.08%, Cr 24.0–26.0%, Ni 19.0–22.0%, Si ≤1.00%, and Mo ≤0.75%—and every route must still pass through the solution anneal required by SA-312.

  • Seamless (SML) — no welding at any stage of manufacture. Seamless is preferred for small-bore furnace and radiant tubing, thick-wall process pipe, and pressure parts when the project specification excludes welded pipe or when piping-class documentation is written around seamless product only. Hot-finished or cold-finished seamless must still be solution annealed to the Table 2 default practice and rapidly cooled.
  • Welded (WLD) — automatic welding without filler metal. The weld is finished so that the pipe meets dimensional and mechanical requirements after the final heat treatment required by SA-312. Welded product is widely used for larger NPS process headers and ducts where the code accepts welded austenitic pipe; the plate heat must itself meet TP310S chemistry.
  • Heavily cold-worked (HCW) — welded pipe that is cold worked to a reduction of area of wall and weld of at least 35% before the final anneal, again without filler metal in the longitudinal weld. The weld is radiographed before cold work. HCW is ordered when the buyer wants tighter OD/wall consistency for exchanger bundles and the process controls written into SA-312 for that route.

Each finished length is hydrostatically tested or nondestructively electrically tested; the manufacturer may choose the method unless the purchase order fixes one. Pipe NPS 10 and larger may ship marked “NH” only when the purchaser agrees to a system test in lieu of hydrotest. Lot definitions follow clause 11.1. Clause 17 heat-treatment lot marking is not mandatory for TP310S (it is not an H grade and not S30815), but heat identity on the stencil and MTC remains required, and buyers often request lot identity for fabrication traceability.

TP310S melt capacity is broader than ASME SA312 UNS S31002 Stainless Steel Pipe or columbium-bearing 310 grades, so lead times for standard schedules are usually shorter. Heavy-wall seamless above Schedule 80XX can still need dedicated rolling slots—state the need date on the enquiry. Dual certification to TP310H is possible only when carbon also meets the 0.04–0.10% H band and grain size is controlled; most commodity 310S heats will not qualify. Where creep or stress-rupture governs, move the conversation to ASME SA312 TP310H Stainless Steel Pipe rather than stretching a non-H heat into an H-grade design basis. Where ultra-low C and Si are mandatory for oxidizing aqueous service, switch to ASME SA312 UNS S31002 Stainless Steel Pipe instead of forcing TP310S into that chemistry window.

Chemical Composition of SA312 TP310S

Two chemistry layers matter: melting (heat / ladle) analysis—mandatory per heat under ASME SA-312/ASTM A312 Table 1—and product analysis when ordered (Suppl. S1 / PO). SA-312/A312 defer product-analysis tolerances through ASTM A999/A999M §6.3 to ASTM A480/A480M Table A1.1. SHH STEEL reports actual ladle and, when ordered, product values—never unpublished tighter windows. Spot-check carbon ≤0.08%, chromium 24–26%, and nickel 19–22% first on receipt; those three values, plus the Mo ≤0.75% residual, are what separate TP310S from neighboring 309 and specialty 310 rows.

Melting analysis (heat / ladle analysis) — Table 1

Heat analysis for Grade TP310S / UNS S31008 from ASME SA-312/SA-312M (ASTM A312/A312M) Table 1 is summarized below. Values are maximum unless a range is shown; ellipses (…) mean no requirement in the ordered edition.

Element TP310S / UNS S31008 melting analysis
Carbon (C) ≤ 0.08
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.030
Silicon (Si) ≤ 1.00
Chromium (Cr) 24.0 – 26.0
Nickel (Ni) 19.0 – 22.0
Molybdenum (Mo) ≤ 0.75

Source: SA-312 Table 1, TP310S / UNS S31008. No nitrogen requirement in Table 1 for this grade.

Chromium drives oxidation resistance; nickel stabilizes austenite and supports toughness at the 25Cr–20Ni balance; the 0.08% carbon ceiling limits sensitization relative to older unrestricted-carbon 310; molybdenum is a residual control, not an alloying addition for pitting resistance. The Mo ≤0.75% ceiling is why 310S is not a chloride-service substitute for TP316/TP316L. Nitrogen is not a Table 1 element for TP310S—mills may still report N as information, but absence of N on the MTC is not a Table 1 nonconformance for this grade (contrast ASME SA312 UNS S31002 Stainless Steel Pipe, where N ≤0.10% is required).

Product analysis — A480/A480M Table A1.1 tolerances applied to Table 1

When product analysis is ordered, finished-pipe chemistry shall meet Table 1 as modified by the product-analysis tolerances of ASTM A480/A480M Table A1.1 (via A999 §6.3). The verified product-analysis limits for TP310S are:

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) ≤ 0.08 0.01 over ≤ 0.09
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.045 0.010 over ≤ 0.055
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) ≤ 1.00 0.05 over ≤ 1.05
Chromium (Cr) 24.0 – 26.0 0.25 under / over 23.75 – 26.25
Nickel (Ni) 19.0 – 22.0 0.15 under / 0.20 over 18.85 – 22.20
Molybdenum (Mo) ≤ 0.75 0.05 over ≤ 0.80

Carbon ≤0.08%: the “S” low-carbon limit that improves weld HAZ resistance versus older high-carbon 310. It is a maximum only—do not confuse with TP310H’s 0.04–0.10% band. Vs UNS S31002: TP310S allows C ≤0.08 (vs ≤0.015), Si ≤1.00 (vs ≤0.15), Mo ≤0.75 (vs ≤0.10), P ≤0.045 / S ≤0.030 (vs 0.020 / 0.015), and has no N max in Table 1. Vs TP309S: higher Cr (24–26 vs 22–24) and Ni (19–22 vs 12–15); same C ≤0.08 and Mo ≤0.75 pattern. Product Cr uses the 0.25 under/over band; Ni uses 0.15 under / 0.20 over (10–20% / 20–30% rows). Mo product tolerance is 0.05 over at the 0.75% max, so product Mo ≤0.80% is established without a special agreement (unlike S31002’s Mo ≤0.10% A480 gap).

Element TP310S TP310H TP310Cb UNS S31002
C ≤ 0.08 0.04 – 0.10 ≤ 0.08 ≤ 0.015
Si ≤ 1.00 ≤ 1.00 ≤ 1.00 ≤ 0.15
Mo ≤ 0.75 … ≤ 0.75 ≤ 0.10
Nb … … 10×C – 1.10 …
N … … … ≤ 0.10
H controls No Yes No No

The side-by-side table above shows why a shared “310” or “310S” market label is dangerous: ASME SA312 TP310H Stainless Steel Pipe adds H-grade carbon and grain rules; ASME SA312 TP310Cb Stainless Steel Pipe stabilizes with niobium; ASME SA312 UNS S31002 Stainless Steel Pipe combines ultra-low C with ultra-low Si and Mo; TP310S is the commodity workhorse row with C ≤0.08% and Si ≤1.00%. Do not invent Table 1 maxima for Ti, Nb, Cu, or Al on TP310S. Residual elements not listed in Table 1 are controlled by melt practice and by any purchase-order limits the buyer adds.

Mechanical Properties of SA312 TP310S

Room-temperature tensile requirements for TP310S / UNS S31008 come from ASME SA-312/ASTM A312 Table 4. Low carbon improves welded corrosion behaviour; it does not change the room-temperature tensile floor, which matches TP309S and most other non-H 300-series SA-312 grades. Actual mill values are often higher than the minima, but design still uses Table 4 for ambient checks and the governing code allowables for elevated-temperature design of S31008.

Property TP310S (S31008)
Tensile strength, min 75 ksi [515 MPa]
Yield strength, min 30 ksi [205 MPa]
Elongation 35% longitudinal / 25% transverse
Hardness No Table 4 maximum

Source: SA-312 Table 4 for TP310S / UNS S31008. These floors match ASME SA312 TP309S Stainless Steel Pipe; ASME SA312 UNS S31002 Stainless Steel Pipe is lower at 73 ksi tensile. Elongation follows the Table 4 row for the ordered edition. No Table 5 grain-size requirement (not an H grade).

Base mechanical testing includes tension on a lot basis and flattening (or the alternate bend where the standard permits) typically on 5% of the lot, plus hydrotest or NDE on every length. Elevated-temperature tensile and rupture tests are purchase-order options, not base SA-312 requirements. For pressure-retaining parts, use the governing Section II Part D or project-code allowables for UNS S31008—do not invent values, and do not copy TP304 or TP316 stress tables into a TP310S calculation package. Copying TP310H tables may also be wrong when the code separates H and non-H entries.

Although Table 4 has no hardness maximum, fabricators sometimes set a Rockwell limit for bending or expanding—put any such limit on the PO and verify it on the MTC if required. Like other 310 grades, TP310S hardens when cold worked; intermediate anneals may be needed for severe forming, and those anneals must still meet the Table 2 default practice. After long high-temperature service, expect reduced room-temperature ductility from carbides and possible sigma—evaluate before cold repair. For creep-range service, see ASME SA312 TP310H Stainless Steel Pipe rather than stretching a non-H heat into an H-grade application.

Dimensions and Tolerances

Dimensional supply for SA312 TP310S pipe follows ASME B36.19 schedules for common NPS/schedule combinations, with special OD and wall by agreement when furnace tubes, radiant coils, or process heaters need a non-standard section. Outside-diameter variations follow ASTM A999/A999M; wall-thickness variations follow SA-312 Table 3 as summarized below. State whether wall is nominal or minimum (Suppl. S8) on the purchase order so the mill does not ship the wrong interpretation.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

Source: SA-312 Table 3; outside diameter variations per A999/A999M.

  • Lengths — NPS 1/8–8 commonly furnished up to 24 ft unless otherwise agreed; SRL, DRL, or cut-to-length on order
  • Cut lengths — never short; typically ≤1/4 in. [6 mm] over unless the PO states a tighter band
  • Ends — plain or beveled; confirm bevel angle and root face when the WPS is already frozen. Threaded TP310S is uncommon for high-temperature service

Furnace and radiant coils often need non-standard walls. Special OD × wall combinations should state whether the wall is minimum under tolerance or nominal before the pierce and roll sequence is set. Straightness, end finish, and length tolerance should be written explicitly for export projects so receiving inspection has a clear acceptance basis. For socket-weld or threaded ends on thin schedules, confirm the wall remains adequate after the 12.5% under-tolerance. Jointers are not permitted unless the purchase order expressly allows them; cut-to-length programmes should include an allowance for fit-up scrap so the mill does not ship under-length pieces. Mass tolerance, OD, and wall bands follow the same A999/Table 3 framework used for other SA-312 austenitics.

Equivalent Grades

Equivalence for TP310S is primarily an ASME/ASTM identity question. The governing pipe designation is ASME SA-312 TP310S / UNS S31008; market names and plate counterparts must be mapped back to that row before a mill is asked to dual-mark or substitute.

Designation Notes
SA-312 / A312 TP310S / UNS S31008 Governing for this pack
ASTM A312 TP310S Identical chemistry when editions align
EN 1.4845 (X8CrNi25-21) approx. Engineering map only—recheck limits
JIS SUS 310S Similar intent; verify C and Si
SA-240 / A240 S31008 Plate/sheet counterpart when listed—not a pipe specification by itself

Related SA-312 grades on steelspecs.com: ASME SA312 TP310H Stainless Steel Pipe, ASME SA312 UNS S31002 Stainless Steel Pipe, ASME SA312 TP310Cb Stainless Steel Pipe, ASME SA312 TP310HCb Stainless Steel Pipe, ASME SA312 TP309S Stainless Steel Pipe, ASME SA312 TP309H Stainless Steel Pipe, ASME SA312 UNS S30815 Stainless Steel Pipe. Versus ASME SA312 TP310H Stainless Steel Pipe, TP310S lacks H-grade carbon and grain controls—do not substitute without reviewing the design-code creep basis. Versus ASME SA312 UNS S31002 Stainless Steel Pipe, TP310S is the commodity row with higher C/Si ceilings and a 75 ksi floor. Versus ASME SA312 TP309S Stainless Steel Pipe, TP310S carries higher Cr and Ni for hotter oxidation service. Versus ASME SA312 UNS S30815 Stainless Steel Pipe, TP310S lacks the intentional silicon and rare-earth additions that S30815 uses for high-temperature strength. EN 1.4845 and JIS SUS 310S are frequently cited as “equivalents,” but those standards can differ in carbon, silicon, and residual limits—a heat that meets EN 1.4845 may still fail SA-312 Table 1 for Mo or S, and vice versa. Dual certification is a mill judgment documented on the MTC—not an automatic entitlement.

Heat Treatment and Delivery Condition

TP310S / S31008 is not individually listed in SA-312 Table 2, so the grade follows the Table 2 default of 1900 °F [1040 °C] minimum with rapid cooling. Because TP310S is not an H grade, clause 6.2 reheat language does not apply and direct quench after hot forming is accepted. There is no Table 5 grain-size rule. Delivery remains the solution-annealed condition required by SA-312 unless the ordered edition and purchase order state otherwise.

  • Solution anneal ≥1900 °F [1040 °C] — Table 2 default; rapid cool
  • No Table 5 grain-size rule — not an H grade
  • Clause 17 lot marking — not mandatory for TP310S; often requested for traceability
  • Free of scale and exogenous iron — descaled / pickled or equivalent as ordered
  • Bright anneal / passivation — available on request when the end-user specification requires a scale-free or passivated surface

Annealing at the Table 2 default dissolves residual carbides and restores corrosion resistance after hot work; rapid cooling is required. Bright annealing under hydrogen or vacuum can deliver a scale-free surface; pickled finishes are acceptable when fully rinsed. If a project wants H-grade grain control on a 310 chemistry, order ASME SA312 TP310H Stainless Steel Pipe instead and accept the carbon minimum and lot-marking rules. Mills may still choose to re-anneal for straightness or surface reasons; that is practice, not an SA-312 H-grade rule. Cite the ordered edition’s Table 2 default practice on the enquiry so the mill does not apply a neighboring H-grade reheat habit to a TP310S heat by mistake.

Corrosion Resistance

TP310S combines 310-level hot oxidation resistance with low-carbon weldability for intermittent aqueous exposure. Chromium at 24.0–26.0% supports continuous service in air and many furnace atmospheres at temperatures where 304/316 scale rapidly; carbon ≤0.08% reduces sensitization risk in the weld heat-affected zone versus older high-carbon 310. SA-312 itself publishes no corrosion rates—service claims need engineering review against the actual gas or liquid chemistry.

  • High-temperature oxidation — 24–26% Cr supports hot-air and flue-gas duty where classic 18-8 grades scale rapidly; industry handbooks often rate intermittent air service into the 1900–2100 °F range, but always defer to the design code’s temperature limits for S31008
  • Intergranular corrosion — C ≤0.08% reduces chromium-carbide sensitization risk in the HAZ versus unrestricted-carbon 310
  • Aqueous chlorides — Mo ≤0.75% residual—not a duplex or 316 substitute for seawater or concentrated chloride service
  • Carburizing / sulfidizing gases — evaluate case by case; ASME SA312 UNS S30815 Stainless Steel Pipe or other specialty grades may be preferred for intentional high-silicon / rare-earth service
  • Sigma-phase risk — high-Cr grades can form sigma after long intermediate-temperature exposure; design dwell times accordingly

Verify intergranular resistance with Suppl. S7 (ASTM A262 Practice E) when aqueous exposure after welding is critical. For nitric-acid or other oxidizing aqueous duties that demand Si ≤0.15% and C ≤0.015%, specify ASME SA312 UNS S31002 Stainless Steel Pipe rather than TP310S. In carburizing atmospheres, 310S can form a chromium-depleted zone over long exposures; in sulfidizing gases, nickel sulfides can form—evaluate carefully with the project corrosion engineer. Compared with ASME SA312 TP309S Stainless Steel Pipe, TP310S offers higher Cr/Ni for hotter oxidation; compared with ASME SA312 UNS S31002 Stainless Steel Pipe, TP310S trades the ultra-low C/Si aqueous advantage for broader melt availability and the higher 75 ksi tensile floor.

Applications of SA312 TP310S Pipe

Buyers typically select TP310S when the project needs 25Cr–20Ni hot-gas oxidation resistance, low-carbon weldability for intermittent aqueous exposure, and commodity availability that specialty rows such as S31002 or TP310HCb cannot match. The grade earns its keep as the workhorse 310 pipe for furnace, radiant, and hot-process duty.

Application Why TP310S Caution
Furnace tubes and radiant coils 25Cr-20Ni oxidation resistance Consider TP310H for creep-critical design
Heat-exchanger shells and headers Low-C weldability + hot strength Chloride waters need different alloys
Hot process and flue-gas ducts Scale resistance, commodity availability Sulfidation may need specialty grades
Refinery and petrochemical heaters Common 310S stock sizes Confirm design code allowables for S31008
Welded process piping with intermittent aqueous exposure C ≤0.08% limits HAZ sensitization Order S7 if proof is required

When creep rupture life governs, move to ASME SA312 TP310H Stainless Steel Pipe. When ultra-low C/Si is mandatory, move to ASME SA312 UNS S31002 Stainless Steel Pipe. When welded HAZ integrity is the driver but niobium stabilization is preferred over low carbon alone, compare ASME SA312 TP310Cb Stainless Steel Pipe. When 310-level Cr/Ni is not required, ASME SA312 TP309S Stainless Steel Pipe is often the more economical choice. Enquiry packages for TP310S should list design temperature, medium (air, flue gas, process fluid), whether field welding will occur, and whether Supplementary Requirement S7 intergranular testing is required—adding S7 after the heat is poured often delays shipment. Stockists commonly hold NPS 1–6 Schedule 10S/40S TP310S; exotic schedules and seamless heavy wall are more often mill-direct. When replacing TP309S with TP310S in an existing unit, review weld procedures and filler selections—the base-metal change alone does not update the WPS.

Weldability

TP310S welds with GTAW, GMAW, SMAW, and SAW using practices familiar to fabricators of other 310 grades. Low carbon improves as-welded intergranular resistance in the heat-affected zone relative to older high-carbon 310. Mill WLD and HCW longitudinal welds are autogenous (no filler); Table 6 guidance applies to joining with filler, not to the mill seam.

Filler and Table 6: the extracted SA-312 Table 6 shows an ellipsis (“…”) for the matching AWS filler class of TP310S / S31008. Filler selection is therefore by agreement—commonly ER310 / E310-type consumables in shop practice—and must be recorded on the WPS, not asserted here as a Table 6 mandate. Freeze the AWS (or EN) class on the WPS/PQR before production welds.

  • Moderate heat input; clean joints free of oil, paint, and exogenous iron
  • Argon or argon-helium shielding and backing gas for GTAW root passes
  • Remove heat tint; pickle when aqueous service follows
  • Mill seams autogenous; clause 15 repairs must identify any filler used
  • Avoid carbon-steel tooling contamination that seeds free-iron rust

Qualify welding procedures to ASME Section IX on TP310S or matching S31008 chemistry. A PQR on ASME SA312 TP304 Stainless Steel Pipe or TP316 without amendment ignores the higher Cr/Ni balance and the different solidification behaviour of 25-20 weld metal. Dissimilar welds of TP310S to carbon steel still commonly use 309-type fillers for dilution control; capture buttering and dilution decisions in the WPS. After high-temperature service exposure, clean thoroughly before repair welding and follow producer guidance for 310 repair practice. Hydrostatic testing or nondestructive electric testing is applied to each TP310S length under SA-312 and A999 after mill manufacture.

Surface Finishes

Surface condition for SA312 TP310S pipe is stated on the purchase order. Typical mill finishes available from SHH STEEL supply include the following options:

  • Annealed and pickled (AP) — solution annealed, descaled in acid pickle or an equivalent process, producing a matte gray finish common for process and furnace pipe
  • Blasted and pickled — often used for heavy-wall seamless where scale removal benefits from blast first
  • Bright annealed (BA) — annealed in a protective atmosphere to a brighter, scale-free surface where the order allows and mill capability exists for the size; temperature must still meet the Table 2 default
  • As-annealed light oxide — sometimes accepted for furnace parts by agreement when the protective scale will form in service anyway
  • Mechanically polished — grit or Ra-controlled polish on OD and/or ID when ordered; polishing does not replace solution annealing
  • Bead-finished welded OD — weld bead rolled or ground flush as agreed for WLD/HCW product

Passivation after pickle or polish can be added when the end-user specification requires it—SA-312 itself does not mandate passivation. Pre-oxidation—heating new parts in air before exposure to process gas—is sometimes used to build an initial chromia scale; it is a user practice, not an SA-312 delivery condition. For high-temperature service the protective scale forms in operation; the delivered finish mainly affects inspection and cleanliness. Avoid marking materials with low-melting metals or high halide content. End preparation (plain or beveled) should be ordered together with finish so that bevel faces and ID cleanliness meet the same acceptance language. State finish, passivation, and any ink restriction on the order so the mill does not ship a default AP finish into a BA or polished requirement.

Inspection and Testing

Base inspection and testing for SA-312 TP310S pipe combines chemistry, mechanical, and integrity checks. The following items form the usual acceptance package; supplementary requirements apply only when written on the purchase order.

  • Heat (melting) analysis — mandatory per heat against Table 1 for TP310S (UNS S31008), including C ≤0.08%, Cr 24.0–26.0%, Ni 19.0–22.0%, Si ≤1.00%, and Mo ≤0.75%
  • Product analysis — when ordered (Suppl. S1 / purchase-order language), using A480 Table A1.1 tolerances via A999 §6.3
  • Tension test — Table 4 tensile, yield, and elongation on a lot basis (75/30 ksi minima)
  • Flattening test — or alternate bend where the standard permits (typically on 5% of the lot)
  • Hydrostatic test or nondestructive electric test — each length; manufacturer’s option unless the order fixes the method
  • Visual and dimensional check — against ordered NPS/schedule or OD/wall and the applicable tolerance clauses; confirm TP310S / UNS S31008 on every stencil

Mill test certificates: EN 10204 3.1 is the standard documentation package from SHH STEEL supply. The certificate should report all Table 1 elements including Mo as a maximum. EN 10204 3.2 or third-party witness (SGS, Bureau Veritas, TÜV, or the buyer’s nominated agency) is arranged when specified and should be booked before final testing. Dual ASME SA-312 / ASTM A312 certification is available when chemistry, heat treatment, mechanical tests, and marking satisfy the edition(s) named on the order.

Option Purpose
S1 Product analysis A480 A1.1 check on finished pipe
S5 Radiography Weld integrity on WLD pipe
S7 Intergranular When aqueous exposure after welding is critical
S8 Minimum wall Wall interpreted as minimum rather than nominal
OES / PMI Confirm Cr, Ni, Mo; C by combustion if required

Receiving review should confirm Cr 24–26, Ni 19–22, C ≤0.08, Mo ≤0.75, tensile ≥75 ksi, yield ≥30 ksi, elongation, and hydro or NDE method. Hardness is not a Table 4 release criterion unless the PO adds it. PMI that only checks Cr and Ni is a useful receiving screen but does not replace the full heat analysis—guns that miss carbon cannot prove the heat is TP310S rather than a high-carbon 310. Third-party inspectors should verify that the grade stencil reads TP310S / S31008—not merely “310SS” or “25-20.” Keep heat numbers on cut pieces for MTC traceability through fabrication.

Packaging and Shipping

Export and domestic shipments of SA312 TP310S pipe are packed for handling and ocean or land transport. Typical packing practices from SHH STEEL supply include:

  • Seaworthy bundles — pipes strapped or cradled in bundles sized for container or break-bulk handling, with non-metallic separators where needed to protect finish; cradles for heavy lengths
  • End caps / protectors — plastic or metal caps on plain or beveled ends to reduce damage and contamination during transit
  • Marking — durable marking of specification, grade (TP310S), UNS S31008, heat number, size (NPS or OD × wall / schedule), manufacturing type (SML / WLD / HCW), test letters, and mill identity as required by SA-312 and the purchase order
  • Export packing — waterproof wrapping or desiccant as agreed for polished or bright-annealed finishes; container stuffing photos on request

Segregate TP310S from ASME SA312 UNS S31002 Stainless Steel Pipe, ASME SA312 TP310H Stainless Steel Pipe, ASME SA312 TP310Cb Stainless Steel Pipe, and ASME SA312 TP309S Stainless Steel Pipe on the packing list and in the yard so stencil mix-ups do not travel with the shipment—chemistry and mechanical floors differ, and mix-ups discovered after fabrication are expensive. Receiving inspectors should compare stencil heat numbers against the MTC for every length and verify that C ≤0.08%, Cr 24–26%, Ni 19–22%, and Mo ≤0.75% are reported before release to fabrication. Long furnace tubes need intermediate supports in transit to prevent bending and ovality. Keep interiors dry and capped so chloride-bearing moisture does not stain or pit the surface before installation. Shipment docs typically include packing list, invoice, B/L or AWB, and MTC (3.1 or 3.2), plus origin/customs papers per Incoterms. State destination, packing preference, and extra marking at enquiry.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless plate and pipe. For ASME SA312 TP310S / UNS S31008 we quote against the edition you name, report the full Table 1 window on the MTC—including C ≤0.08%, Cr 24.0–26.0%, Ni 19.0–22.0%, Si ≤1.00%, and the Mo ≤0.75% residual—and keep heat identity unbroken from melt through finished length. Receiving inspection then clears the heat against Table 1 and Table 4 rather than against a vague “310S” or “25-20” catalog sheet. We also stay honest about Table 6: no AWS filler class is listed for TP310S, so filler selection stays by agreement on the WPS. Dual 310S/310H options are flagged only when carbon, anneal, and grain-size rules actually allow—we do not pretend commodity 310S heats automatically meet H-grade controls.

  • Specification fidelity — chemistry and tensile to SA-312/A312 Table 1 and Table 4 for TP310S (S31008), not unpublished tighter windows; Mo residual reported
  • Mill resources — SML, WLD, and HCW from qualified stainless pipe mills with heat traceability; cutting and beveling on confirmed orders
  • Documentation — EN 10204 3.1 MTCs standard; 3.2 or third-party inspection on request
  • Dual marking — ASME SA-312 and ASTM A312 when the heat and tests meet both requirements you name; dual 310S/310H when carbon, anneal, and grain-size rules allow
  • Related grades — sister 310-family and 309S SA-312 grades when projects buy matched high-temperature packages
  • Export packing — seaworthy bundles, end protectors, and durable grade/heat/size/type marking

Quotations follow your purchase-order language for edition year, manufacturing type, size, finish, and any supplementary tests you name (S1, S5, S7, S8). Ask for dual 310S/310H options when the design temperature is near the creep boundary, and ask for S31002 when the corrosion case actually needs Si ≤0.15% and C ≤0.015%. Grade hub: ASME SA 312/SA 312M.

Supply Capability

SHH STEEL can supply ASME SA312 TP310S / UNS S31008 stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade.

Item SHH STEEL capability for TP310S
Standard ASME SA-312/SA-312M and/or ASTM A312/A312M Grade TP310S (UNS S31008)
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD/wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length SRL, DRL, or cut-to-length
Finish Annealed and pickled; blasted and pickled; bright annealed or polished by agreement
Testing Tension, flattening/bend, hydro or NDE per length; supplementary tests on order
Documents EN 10204 3.1; third-party inspection / 3.2 on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

TP310S is a regular mill grade with broader melt capacity than S31002 or columbium-bearing 310 variants. Common sizes are often available from stock or short mill runs; heavy walls and special OD/wall combinations are mill-order items with longer lead times. Stock moves with mill rolling cycles. Enquiries should state the SA-312 edition, TP310S / UNS S31008, SML/WLD/HCW, NPS or OD×wall (nominal or minimum), length practice, finish, and any product-analysis or 3.2 requirements so mill slots align with your need date. Cut lengths, beveling, and packing-list marking are available on confirmed orders. Combining project sizes into one heat improves chemistry consistency and helps meet mill minima without over-ordering. If the design temperature sits in the creep range, ask whether TP310H (or dual 310S/310H) is preferred before finalising the PO—changing after mill production is costly. If the corrosion case needs Si ≤0.15% and C ≤0.015%, switch the enquiry to UNS S31002 rather than forcing TP310S into that window.

FAQ

Is ASME SA312 the same as ASTM A312?
For chemistry (Table 1), tensile (Table 4), manufacturing types, and most testing language, ASME SA-312/SA-312M matches ASTM A312/A312M of the referenced edition. Dual SA312/A312 marking is common when ordered. Name both editions on the purchase order and mill test certificate so inspectors can verify the heat against the exact books you cited—do not assume a bare market grade stamp covers dual certification.
What is the UNS number for TP310S?
Table 1 lists TP310S as UNS S31008. Use that UNS on the purchase order, stencil, and MTC so chemistry and tensile rows stay unambiguous against neighboring 310 grades. When the project mixes plate and pipe, carry the same UNS language across forms, but still order pipe to SA-312/A312—not to the plate specification alone.
TP310S vs TP310H — which should I order?
TP310H adds C 0.04–0.10%, Table 5 grain size, and clause 6.2 reheat; TP310S has C ≤0.08% without those H mandates. Both use 75/30 ksi Table 4 floors. Put the design-code grade and UNS on the datasheet and purchase order before you compare price—switching to TP310H after fabrication drawings are frozen usually means a material change notice, not a free mill substitution.
TP310S vs UNS S31002 — which should I order?
UNS S31002 tightens C to ≤0.015%, Si to ≤0.15%, Mo to ≤0.10%, adds N ≤0.10%, and carries a 73 ksi tensile floor. TP310S allows C ≤0.08%, Si ≤1.00%, Mo ≤0.75%, and 75/30 ksi. Order S31002 only when the ultra-low C/Si chemistry is required—commodity 310S heats will never meet S31002. Put the design-code grade and UNS on the purchase order before you compare price.
TP310S vs TP309S — which should I order?
TP310S has higher Cr (24–26%) and Ni (19–22%) than TP309S (22–24% Cr, 12–15% Ni) for stronger high-temperature oxidation resistance. Both share C ≤0.08%, Mo ≤0.75%, and 75/30 ksi floors. Put the design-code grade and UNS on the datasheet and purchase order before you compare price—switching after fabrication drawings are frozen usually means a material change notice, not a free mill substitution.
TP310S vs TP310Cb — which should I order?
TP310Cb adds niobium stabilization (Nb 10×C min to 1.10% max) on the same 25Cr–20Ni base with C ≤0.08%. TP310S has no Nb requirement and relies on the low-carbon ceiling alone for welded HAZ integrity. Choose Nb stabilization or low-carbon 310S based on the corrosion and welding case—they are not drop-in substitutes. Put the design-code grade and UNS on the purchase order before you compare price.
Seamless vs welded TP310S — which is better?
Neither is universally better. Choose the manufacturing type your design code and datasheet allow; both are legitimate SA-312 forms when tested to the standard. State SML, WLD, or HCW on the purchase order and confirm the same letters on the pipe marking and MTC—mixing offers that differ only in manufacturing type is a common bid-evaluation trap.
Can you dual-certify SA312 / A312 TP310S?
Yes, when heat analysis, heat treatment, mechanical tests, and marking meet both editions named on the order. Write the ASME and ASTM edition years on the PO, and require the MTC to reference both books so receiving inspection can clear the heat without a second paperwork chase after shipment. Dual marking with TP310H needs the H-grade carbon band and grain-size rules as well—most commodity 310S heats will not qualify.
Hydrostatic test vs NDE — which do I get?
Each length is hydrotested or nondestructively electrically tested. Manufacturer may choose unless the purchase order fixes the method. If your piping class or client specification locks one method, state it on the PO and verify the chosen test appears on the MTC for every length—silent mill option is not the same as an approved project method.
What heat treatment / anneal temperature applies to TP310S?
Table 2 does not list TP310S individually—use the 1900 °F [1040 °C] default minimum with rapid cooling. It is not an H grade, so clause 6.2 reheat and Table 5 grain size do not apply; direct quench after hot forming is accepted. Delivery remains the solution-annealed condition required by SA-312 unless the edition and PO state otherwise. Cite the ordered edition’s Table 2 default on the enquiry so the mill does not apply a neighboring grade’s anneal practice by habit.
What Table 1 chemistry defines TP310S?
Table 1: C ≤0.08%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 24.0–26.0%, Ni 19.0–22.0%, Mo ≤0.75%; no nitrogen requirement (UNS S31008). Values are melting-analysis limits from the ordered edition—do not invent tighter catalog windows. When product analysis is needed, order it explicitly (Suppl. S1 / PO language) rather than assuming ladle values alone will satisfy receiving inspection.
What are the Table 4 tensile requirements for TP310S?
Table 4 minima are 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield (elongation 35% longitudinal / 25% transverse). Actual MTC values are often higher; design still uses Table 4 unless the PO states higher guarantees. Record the Table 4 row on the datasheet so fabricators do not substitute a sister-grade strength line from memory—UNS S31002 is lower at 73 ksi tensile, and H-grade allowables may differ at elevated temperature.

Conclusion

ASME SA312 TP310S (UNS S31008) is the workhorse low-carbon 25Cr–20Ni stainless steel pipe grade in SA-312: C ≤0.08%, Cr 24.0–26.0%, Ni 19.0–22.0%, Si ≤1.00%, Mo ≤0.75%, Table 4 minima 75/30 ksi, and a Table 2 default 1900 °F [1040 °C] anneal. It is not an H grade and carries no Table 5 grain-size rule. It is not a drop-in for UNS S31002 (ultra-low C/Si, 73 ksi), TP310H (H-grade creep controls), TP310Cb (Nb stabilization), or TP309S (lower Cr/Ni)—each has its own Table 1 row. Table 6 lists no AWS filler class (filler by agreement). Order the manufacturing type (SML/WLD/HCW), schedule or wall, finish, and any product analysis or supplementary tests explicitly. For stock checks, mill certificates, or dual SA-312/A312 supply questions, contact SHH STEEL at admin@steelspecs.com or browse the ASME SA 312/SA 312M category on steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X