ASME SA312 UNS S35045 Stainless Steel Pipe | ASME SA312 Stainless Steel - SHH STEEL

ASME SA312 UNS S35045 Stainless Steel Pipe | SA 312/SA 312M

ASME SA312 UNS S35045 (no TP) high-Cr/Ni Ti+Al stainless steel pipe in SML, WLD and HCW, with Cr 25–29%, Ni 32–37%, Ti/Al 0.15–0.60%, a 70/25 ksi Table 4 floor and a 1900 °F default anneal, supplied by SHH STEEL with EN 10204 3.1 MTCs.
Grade
UNS S35045
Standard
ASME SA312 / SA 312M (ASTM A312 / A312M)
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA312 UNS S35045 Stainless Steel Pipe

ASME SA-312/SA-312M covers seamless, welded, and heavily cold-worked austenitic stainless steel pipe for high-temperature and general corrosive service. UNS S35045 is listed in Table 1 with no TP designation, so it is ordered, marked, and certified by UNS number alone. It is a high-chromium, high-nickel austenitic grade with intentional titanium and aluminum additions: C 0.06–0.10%, Mn ≤1.50%, S ≤0.015%, Si ≤1.00%, Cr 25.0–29.0%, Ni 32.0–37.0%, Ti 0.15–0.60%, Cu ≤0.75%, and Al 0.15–0.60%. Molybdenum, niobium, and nitrogen show as ellipses (no requirement) in the extracted Table 1 row.

Table 4 sets 70 ksi [485 MPa] tensile and 25 ksi [170 MPa] yield as a single row, with the standard 35% longitudinal / 25% transverse elongation pattern unless the ordered edition notes otherwise. Table 2 does not list S35045 individually, so the default solution anneal of 1900 °F [1040 °C] minimum with rapid cooling applies. Table 6 in the extracted edition assigns no AWS filler class, so filler is by agreement. It is not an H grade: there is no Table 5 grain-size mandate and no clause 6.2 reheat. Engineers usually specify it where the high Cr–Ni matrix plus Ti/Al additions are written into the owner material specification for elevated-temperature or specialty process service.

SHH STEEL can supply ASME SA312 UNS S35045 stainless steel pipe to the edition named on the enquiry, in seamless (SML), welded (WLD), and heavily cold-worked (HCW) form. We quote ASME B36.19 schedules and special OD/wall by agreement, ship with EN 10204 3.1 mill test certificates that report every Table 1 element with Ti and Al as actual values, state the 70/25 ksi results and the 1900 °F anneal, and offer dual SA-312/A312 marking when chemistry, heat treatment, mechanical tests, and marking satisfy both editions on the purchase order. Please confirm NPS, wall or schedule, finish, length practice, filler basis, and any product-analysis extras when you enquire.

The list below shows how the names used in the market map to what should appear on the order and certificate. Trade names are useful shorthand, but only the UNS number carries the Table 1 and Table 4 rows.

  • ASME SA312 UNS S35045 / SA-312 Grade UNS S35045 — the marking language for ASME-code and dual-marked pipe
  • ASTM A312 UNS S35045 — same chemistry and tensile tables when the ASTM edition is referenced
  • High-Cr/Ni Ti+Al austenitic (no TP name) — informal description only; insist on UNS S35045 on stencil and MTC

Sister grades buyers compare with S35045 include ASME SA312 UNS S35315 Stainless Steel Pipe (Si–N–Ce high-Ni/Cr with welded 94/39 / seamless 87/38 ksi and a 2010 °F anneal) and ASME SA312 TP310S Stainless Steel Pipe / ASME SA312 TP310H Stainless Steel Pipe (25Cr–20Ni without the Ti/Al window). None of these is a drop-in replacement for S35045. Grade hub: ASME SA 312/SA 312M.

Manufacturing Types (SML / WLD / HCW)

ASME SA-312 recognizes three manufacturing routes for UNS S35045 pipe, and the route is a purchase-order decision driven by the design code, the size range, wall thickness, and how the owner wants the pipe inspected. The route never changes the chemistry: whichever way the pipe is made, the heat must still meet C 0.06–0.10%, Cr 25.0–29.0%, Ni 32.0–37.0%, Ti 0.15–0.60%, Al 0.15–0.60%, Mn ≤1.50%, S ≤0.015%, Si ≤1.00%, Cu ≤0.75%, and every length must still go through the solution anneal at the default 1900 °F [1040 °C] minimum before it is released.

  • Seamless (SML) — no welding at any stage. Preferred for high-pressure service, thick walls, and owners who exclude welded pipe from the design class. Seamless suits high-pressure and heavy-wall lines where welded pipe is excluded from the class.
  • Welded (WLD) — automatic welding without filler metal, with the weld finished so the pipe meets dimensional and mechanical requirements after the final heat treatment. The strip or plate heat must itself carry the full UNS S35045 chemistry, so ask for the coil or plate heat number on the certificate.
  • Heavily cold-worked (HCW) — welded pipe cold worked to at least 35% reduction of wall and weld before the final anneal, again without filler in the longitudinal seam, with the weld radiographed before cold work. Order HCW when the project specifically wants that marking and the process controls SA-312 writes around it.

Every finished length is hydrostatically tested or nondestructively electrically tested, and the mill may choose the method unless the purchase order fixes one. Pipe NPS 10 and larger may ship marked “NH” only when the purchaser accepts a system test in place of the hydrotest, and lots for mechanical testing follow clause 11.1. Clause 17 heat-treatment lot marking is not mandatory because S35045 is not an H grade, but projects buying this alloy almost always want heat and lot identity on the stencil. Dual certification to S35315 or TP310S is not possible because the chemistry windows do not overlap.

S35045 is an uncommon SA-312 listing and is essentially always made to order. Lead times follow specialty melt schedules, so enquire early with route, sizes, wall, Ti/Al reporting, filler basis, and any product-analysis extras.

Chemical Composition of SA312 UNS S35045

Two chemistry layers matter for UNS S35045. The melting (heat or ladle) analysis is mandatory for every heat under SA-312/A312 Table 1, while product analysis on finished pipe applies only when it is ordered through Supplementary Requirement S1 or purchase-order wording. Product tolerances are not printed in SA-312 itself; they come through ASTM A999/A999M §6.3 from ASTM A480/A480M Table A1.1. SHH STEEL reports the actual ladle values and, when ordered, the product values, and never quotes tighter catalogue windows that the standard does not publish.

Melting analysis (heat / ladle analysis) — Table 1

Heat analysis for UNS S35045 from ASME SA-312/SA-312M (ASTM A312/A312M) Table 1 is summarized below. Values are maximum unless a range is shown, and an ellipsis (…) means the ordered edition sets no requirement for that element.

Element UNS S35045 melting analysis
Carbon (C) 0.06 – 0.10
Manganese (Mn) ≤ 1.50
Phosphorus (P) No requirement listed (…) — see UNCERTAIN
Sulfur (S) ≤ 0.015
Silicon (Si) ≤ 1.00
Chromium (Cr) 25.0 – 29.0
Nickel (Ni) 32.0 – 37.0
Molybdenum (Mo) No requirement (…)
Titanium (Ti) 0.15 – 0.60
Copper (Cu) ≤ 0.75
Aluminum (Al) 0.15 – 0.60
Niobium (Nb) No requirement (…)
Nitrogen (N) No requirement (…)

Source: SA-312 Table 1, UNS S35045. The grade column shows “…”, confirming there is no TP name. Phosphorus is listed as “…” in the extracted edition—no numeric max in this pack; confirm in the purchaser’s edition (see UNCERTAIN).

Product analysis — A480/A480M Table A1.1 tolerances applied to Table 1

When product analysis is ordered, finished-pipe chemistry shall meet Table 1 as modified by the tolerances in ASTM A480/A480M Table A1.1. The resulting limits used for UNS S35045 receiving inspection are:

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) 0.06 – 0.10 0.01 under / over 0.05 – 0.11
Manganese (Mn) ≤ 1.50 0.04 over ≤ 1.54
Sulfur (S) ≤ 0.015 0.005 over ≤ 0.020
Silicon (Si) ≤ 1.00 0.05 over ≤ 1.05
Chromium (Cr) 25.0 – 29.0 0.20 under / over 24.80 – 29.20
Nickel (Ni) 32.0 – 37.0 0.15 under / over 31.85 – 37.15
Titanium (Ti) 0.15 – 0.60 0.05 under / over 0.10 – 0.65
Copper (Cu) ≤ 0.75 0.05 over ≤ 0.80
Aluminum (Al) 0.15 – 0.60 0.05 under / over 0.10 – 0.65

The values to check first on receipt are chromium 25.0–29.0%, nickel 32.0–37.0%, titanium 0.15–0.60%, and aluminum 0.15–0.60%, together with the tight sulfur ceiling of 0.015% and manganese ≤1.50%. Carbon sits in a 0.06–0.10% band, which is higher than typical L grades and should not be confused with an H-grade carbon floor. A heat that reports Ti or Al outside the window is not S35045, which is why ordering by a trade description without the UNS is a genuine risk. If product analysis is ordered, state the A480 basis on the purchase order so the mill and the receiving laboratory work from the same limits.

Mechanical Properties of SA312 UNS S35045

Room-temperature tensile requirements for UNS S35045 come from SA-312 Table 4 and are summarized below. These are minimum release values for the lot, not typical values, and design allowables must always be taken from the governing code tables for UNS S35045 rather than from a neighbouring grade.

Property UNS S35045
Tensile, min 70 ksi [485 MPa]
Yield, min 25 ksi [170 MPa]
Elongation 35% L / 25% T (standard Table 4 pattern unless edition notes otherwise)

The 70/25 ksi row applies to all walls, so there is no thickness split to check. Elongation follows the standard Table 4 pattern of 35% longitudinal / 25% transverse unless the ordered edition notes otherwise—confirm that footnote if your inspector’s checklist is edition-sensitive. Table 4 does not set a hardness maximum for S35045. Certificate values are normally above the minima, but the design basis should still use Table 4 and the code allowables unless the mill has accepted higher guaranteed values in writing.

Delivery is the solution-annealed condition. The high-nickel austenitic structure gives good toughness at low temperature, though impact testing remains a project extra rather than part of the SA-312 base package.

Dimensions and Tolerances

Dimensional supply for SA312 UNS S35045 pipe follows ASME B36.19 schedules for the common NPS and schedule combinations, with special OD and wall available by agreement when a project needs a section the schedules do not cover. Outside-diameter variations follow ASTM A999/A999M, and wall-thickness variations follow SA-312 Table 3 as summarized below. State on the purchase order whether wall is nominal or minimum (Supplementary S8), because the two readings produce different pipe from the same size line.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

Source: SA-312 Table 3; outside diameter variations per A999/A999M.

  • Lengths — single random, double random, or cut-to-length on order
  • Cut lengths — typically no more than 1/4 in. [6 mm] over the ordered length unless the PO states a tighter band
  • Ends — plain or beveled; confirm bevel angle and root face when the WPS is already frozen

Many high-alloy buyers order by OD × wall rather than NPS and schedule, which is fine as long as the enquiry says so clearly. Straightness, end finish, and length tolerance should be written into export orders so receiving inspection has an agreed acceptance basis instead of arguing after arrival. On thin schedules with threaded or socket-weld ends, check that the remaining wall is still adequate after the 12.5% under-tolerance. Jointers are not permitted unless the purchase order allows them, so cut-to-length programmes should include an allowance for fit-up scrap rather than expecting the mill to ship short pieces.

Equivalent Grades

UNS S35045 has no TP name in SA-312, and cross-references to proprietary or EN grades are approximate at best. Any mapping has to be checked element by element against Table 1, with particular care on Cr, Ni, Ti, and Al.

Designation Notes
ASME SA-312 / ASTM A312 UNS S35045 Governing pipe product standard — no TP name
UNS S35045 Unified number listed in Table 1
UNS S35315 Si–N–Ce high-Ni/Cr sister; different tensile and anneal rows
TP310S / TP310H 25Cr–20Ni family without the Ti/Al window

Treat trade-name equivalents as commercial shorthand rather than a substitution approval, because a heat can satisfy a trade window and still miss the S35045 titanium or aluminum range. Dual certification is valid only when every Table 1 element passes and the tensile results meet 70/25 ksi. Related SA-312 pages: ASME SA312 UNS S35315 Stainless Steel Pipe, ASME SA312 TP310S Stainless Steel Pipe, ASME SA312 TP310H Stainless Steel Pipe, ASME SA312 TP321 Stainless Steel Pipe. Hub: ASME SA 312/SA 312M.

Pressure-code caution: EN or proprietary approximations do not authorize B31 or Section VIII substitution without engineered approval and an accepted material specification on the design documents.

Heat Treatment and Delivery Condition

All pipe furnished to ASME SA-312 shall be heat treated. UNS S35045 does not carry an individual temperature row in Table 2, so the default minimum solution-annealing temperature of 1900 °F [1040 °C] applies, followed by water quenching or another rapid cool sufficient to prevent harmful carbide reprecipitation. That default is SHH STEEL’s delivery baseline unless the ordered edition states otherwise.

S35045 is not an H grade, so clause 6.2 reheat, Table 5 grain size, and mandatory clause 17 lot marking do not apply. Bright annealing is possible by agreement where the mill can hold temperature in a protective atmosphere for the size. If pipe is hot formed or bent after delivery, plan a full re-anneal at the same practice rather than a stress relief alone, because formed parts carry the same carbide-risk window as straight lengths.

Commercial delivery condition for UNS S35045 typically includes solution annealing to Table 2, pickling or bright annealing as ordered, straightening and cutting to the ordered length practice, and hydrotesting or NDE per length as required by the standard and the purchase order.

Corrosion Resistance

SA-312 does not include a corrosion table, so this section is engineering commentary rather than a guarantee. With Cr 25–29% and Ni 32–37%, S35045 offers a high-alloy austenitic matrix that buyers typically select for elevated-temperature oxidation resistance and general corrosive duty where the owner specification also wants Ti and Al in the stated windows. Titanium can help stabilize carbon; aluminum is often associated with oxidation performance in high-Cr/Ni alloys—but those are engineering interpretations, not SA-312 corrosion guarantees.

  • Elevated-temperature process lines — where high Cr–Ni chemistry is written into the material specification
  • Specialty residual-control packages — when Ti and Al must appear as actual values on the MTC
  • Compared with 310S — higher nickel and intentional Ti/Al rather than a simple 25–20 chemistry

Critical corrosion or oxidation test results depend on surface condition, weld quality, and the test method, so if they matter, write them into the purchase order. Welds are usually the weakest point, which is why agreed fillers and careful post-weld cleaning are standard practice for this grade. Related pages: ASME SA312 UNS S35315 Stainless Steel Pipe, ASME SA312 TP310S Stainless Steel Pipe.

Applications of SA312 UNS S35045 Pipe

Applications for UNS S35045 pipe are driven by the high Cr–Ni matrix and by owner specifications that name Ti and Al in the Table 1 windows. The table below summarizes where buyers typically specify the grade.

Application area Typical use of UNS S35045 pipe Selection note
High-Cr/Ni process or furnace-adjacent lines Elevated-temperature service written around S35045 chemistry Prove Ti and Al on the MTC
Specialty chemical process piping Owner datasheets that name UNS S35045 rather than a TP grade Order by UNS; do not accept a 310S substitute
Code piping packages Dual SA-312/A312 projects with heat traceability Name edition, route, and UNS on the enquiry
Matched high-alloy packages Projects also buying S35315 or 310-family pipe Segregate grades; tensile and anneal rows differ

Before committing, compare the duty against ASME SA312 UNS S35315 Stainless Steel Pipe and ASME SA312 TP310S Stainless Steel Pipe, and confirm the owner specification on filler class, post-weld cleaning, and any corrosion or oxidation testing. For moderate duties, a standard 310 or 321 grade may be enough and easier to source.

Weldability

Table 6 in the extracted edition does not assign an AWS filler class to UNS S35045, so the filler is by agreement. Whatever is chosen, name it specifically on the WPS and PQR and qualify it on S35045 base metal before production welding. Low heat input and controlled interpass remain good practice on this high-alloy austenitic.

  • Qualify on S35045 — not on 310S or 321 coupons
  • Control heat input and interpass temperature — to limit HAZ sensitization and residual-stress issues
  • Back-purge roots — to prevent ID oxidation on corrosion-critical lines
  • Remove heat tint — by pickling or mechanical cleaning where the owner specification requires it

Mill longitudinal welds on WLD and HCW pipe are autogenous, so the filler question applies only to fabrication joints. NDE extent for girth welds is a fabrication-code decision, separate from the mill hydro or electric test on each length.

Surface Finishes

Surface condition for UNS S35045 pipe should be stated on the purchase order rather than left to mill default. For stainless pipe, embedded free iron, residual scale, and chloride-bearing residues are where corrosion starts, so the finish is part of the material performance and not just appearance. The finishes we regularly quote for this grade are listed below.

  • Annealed and pickled (AP) — solution annealed at the default 1900 °F [1040 °C] minimum, then descaled in acid pickle or an equivalent process to a matte grey finish; the standard choice for process pipe
  • Blasted and pickled — common on heavy-wall seamless where blasting first makes scale removal more reliable
  • Bright annealed (BA) — annealed in a protective atmosphere where mill capability exists for the size; the anneal temperature still has to meet the Table 2 practice for UNS S35045
  • Mechanically polished — OD and/or ID polish to an agreed grit or Ra when ordered; polishing never replaces the solution anneal
  • Bead-finished welded OD — weld bead rolled or ground flush as agreed on WLD and HCW product

For S35045 the pickle must remove scale cleanly so residual oxides do not undermine the high-alloy surface in service. Passivation after pickling or polishing can be added when the end-user specification calls for it, even though SA-312 itself does not require it. If the project bans chloride-bearing marking inks, say so on the order; otherwise the mill will apply its normal stencil practice and ship its default AP finish.

Inspection and Testing

The base acceptance package for SA-312 UNS S35045 pipe combines chemistry, tensile testing, heat-treatment evidence, and a pressure or electrical integrity test on every length. The items below make up the usual package; supplementary requirements and project corrosion tests only apply when they are written on the purchase order.

  • Heat (melting) analysis — mandatory per heat against Table 1 for UNS S35045: C 0.06–0.10%, Cr 25.0–29.0%, Ni 32.0–37.0%, Ti 0.15–0.60%, Al 0.15–0.60%, Mn ≤1.50%, S ≤0.015%, Si ≤1.00%, Cu ≤0.75%
  • Product analysis — when ordered (Suppl. S1 or PO wording), using A480 Table A1.1 tolerances via A999 §6.3; note that phosphorus has no numeric Table 1 max in this pack’s extract
  • Tension test — 70 ksi [485 MPa] tensile / 25 ksi [170 MPa] yield (70/25 ksi minima) on a lot basis
  • Flattening test — or the alternate bend test where the standard permits
  • Hydrostatic or nondestructive electric test — every length; manufacturer’s option unless the order fixes the method
  • Visual and dimensional check — against ordered NPS/schedule or OD × wall, with UNS S35045 (no TP name) on every stencil

Mill test certificates: EN 10204 3.1 is the standard documentation from SHH STEEL supply. For S35045 the certificate must report all Table 1 elements with Ti and Al shown as actual values, together with 70/25 ksi tensile results, the hydro or NDE method, and a 1900 °F anneal statement. Confirm the purchaser’s edition for any phosphorus limit. EN 10204 3.2 or third-party witness by SGS, Bureau Veritas, TÜV, or the buyer’s nominated agency is arranged when specified, and it should be booked before final testing rather than after the heat has been released. Dual ASME SA-312 / ASTM A312 certification is available when chemistry, heat treatment, mechanical tests, and marking satisfy both editions named on the order.

Option Purpose
S1 product analysis Confirms chemistry on finished pipe
S5 radiography Weld integrity on WLD pipe
S7 intergranular corrosion A262 Practice E after sensitizing treatment
S8 minimum wall Wall interpreted as minimum rather than nominal
S9 weld decay Compares weld and base-metal loss rates

Receiving review should confirm Cr 25–29, Ni 32–37, Ti 0.15–0.60, Al 0.15–0.60, C 0.06–0.10, S ≤0.015, then 70/25 ksi tensile and the anneal statement. Make sure the stencil reads UNS S35045, not a 310 or trade name.

Packaging and Shipping

Export and domestic shipments of SA312 UNS S35045 pipe are packed for handling and for ocean or land transport. The packing we normally apply is summarized below, and anything beyond it can be agreed on the order.

  • Seaworthy bundles — pipes strapped or cradled in bundles sized for container or break-bulk handling, with non-metallic separators where the finish needs protecting
  • End caps — plastic or metal caps on plain or beveled ends to keep out damage and contamination in transit
  • Marking — specification, grade (UNS S35045 (no TP name)), heat number, size, manufacturing type (SML / WLD / HCW), test letters, and mill identity as SA-312 and the purchase order require
  • Export protection — waterproof wrapping or desiccant as agreed for polished or bright-annealed finishes, with low-chloride inks on request

Segregate UNS S35045 from ASME SA312 UNS S35315 Stainless Steel Pipe and ASME SA312 TP310S Stainless Steel Pipe on the packing list and in the yard, because the grades look identical and a mix-up found after fabrication cannot be corrected by heat treatment. Keep interiors dry and capped so chloride-bearing moisture cannot stain or pit the surface before installation. Shipping documents normally include the packing list, invoice, bill of lading or air waybill, and the 3.1 or 3.2 MTC with full Table 1 chemistry, plus origin and customs papers to suit the agreed Incoterms.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless plate and pipe, and for ASME SA312 UNS S35045 / UNS S35045 we quote against the edition you name rather than a generic catalogue sheet. We report every Table 1 element on the MTC—including Ti 0.15–0.60% and Al 0.15–0.60%—together with the 70/25 ksi Table 4 results and the 1900 °F anneal statement. Heat identity stays unbroken from the melt to the finished length, so receiving inspection can clear each heat against Table 1 and Table 4 without chasing paperwork after the pipe has arrived.

We check supplier certificates before shipment for a missing Ti or Al value, a phosphorus claim that the extract does not support, and paperwork that treats S35045 as interchangeable with 310S. We are also open about what the standard leaves open: Table 6 assigns no filler class, phosphorus is “…” in this pack’s extract, and EN maps are soft.

  • Specification fidelity — chemistry and tensile to SA-312/A312 Table 1 and Table 4 for UNS S35045; Ti/Al reported; 70/25 ksi confirmed; 1900 °F anneal stated
  • Mill resources — SML, WLD, and HCW from qualified stainless pipe mills with heat traceability; cutting and beveling on confirmed orders
  • Documentation — EN 10204 3.1 MTCs as standard with full Table 1 chemistry; 3.2 or third-party inspection on request
  • Dual marking — ASME SA-312 and ASTM A312 when the heat and tests meet both editions you name
  • Related grades — ASME SA312 UNS S35315 Stainless Steel Pipe, ASME SA312 TP310S Stainless Steel Pipe, and ASME SA312 TP310H Stainless Steel Pipe when a project buys a matched package
  • Export packing — seaworthy bundles, end protectors, and durable grade, heat, size, and type marking

Quotations follow your purchase-order language for edition year, manufacturing type, size, wall, finish, and any supplementary tests you name (S1, S5, S7, S8, S9). If the same project also needs plate or fittings, ask for coordinated heats so the chemistry lines up across product forms. Grade hub: ASME SA 312/SA 312M.

Supply Capability

SHH STEEL can supply ASME SA312 UNS S35045 stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade.

Item SHH STEEL capability for UNS S35045
Standard ASME SA-312/SA-312M and/or ASTM A312/A312M UNS S35045 (no TP designation)
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD/wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length SRL, DRL, or cut-to-length
Finish Annealed and pickled; blasted and pickled; bright annealed or polished by agreement
Testing Tension (70/25 ksi), flattening/bend, hydro or NDE per length; Ti/Al/Cr/Ni on MTC; 1900 °F anneal stated; S1/S5/S7/S8/S9 on order; filler by agreement
Documents EN 10204 3.1 with full Table 1 chemistry; third-party inspection / 3.2 on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

UNS S35045 is not a distributor stock grade, so orders are mill runs and lead times follow specialty melt schedules and mill minimums. Enquiries should state the SA-312 edition, UNS S35045 (no TP name), SML/WLD/HCW, NPS or OD × wall (and whether wall is nominal or minimum), length practice, finish, and any product-analysis, corrosion-test, or 3.2 requirements, so mill slots line up with your need date. Cut lengths, beveling, and packing-list marking are available on confirmed orders, and grouping project sizes onto one heat keeps the chemistry consistent while helping meet mill minimums without over-ordering.

FAQ

Is ASME SA312 the same as ASTM A312 for UNS S35045?
For chemistry (Table 1), tensile (Table 4), manufacturing types, and most testing language, ASME SA-312/SA-312M matches ASTM A312/A312M of the referenced edition. Dual SA312/A312 marking is common when ordered. Name both editions on the purchase order and mill test certificate so inspectors can verify the heat against the exact books you cited—do not assume a bare market grade stamp covers dual certification.
Why does UNS S35045 have no TP name?
Table 1 lists S35045 with an ellipsis in the TP column, so the unified number is its only identity in SA-312. Put UNS S35045 on the purchase order, stencil, packing list, and MTC. Labels such as high-Cr/Ni or Ti+Al austenitic are not grade names and can be confused with S35315 or 310-family grades that have different chemistry and tensile rows.
UNS S35045 vs UNS S35315 — which should I order?
S35045 uses Ti 0.15–0.60% and Al 0.15–0.60% on Cr 25–29% / Ni 32–37% with a 70/25 ksi floor and a default 1900 °F anneal. S35315 uses Si 1.20–2.00%, N 0.12–0.18%, and Ce 0.03–0.08% on Cr 24–26% / Ni 34–36%, with welded 94/39 and seamless 87/38 ksi floors and a 2010 °F anneal. The windows do not overlap—order the exact UNS your datasheet names.
UNS S35045 vs TP310S — which should I order?
TP310S is a 25Cr–20Ni grade without the Ti/Al windows and with its own Table 1 and Table 4 rows. S35045 raises nickel to 32–37% and requires Ti and Al in stated bands. They are not interchangeable; order S35045 only when the datasheet names UNS S35045, and do not accept a 310S heat as a substitute.
Seamless vs welded UNS S35045 — which is better?
Neither is universally better. Seamless suits high-pressure and heavy-wall lines, while WLD and HCW are economical for larger diameters and thinner walls when seam quality and the full anneal are controlled. Choose the route your design code and datasheet allow, and confirm the same SML, WLD, or HCW letters on the marking and MTC.
Can you dual-certify SA312 / A312 UNS S35045?
Yes, when the heat analysis, heat treatment, mechanical tests, and marking meet both editions named on the order. Write the ASME and ASTM edition years on the purchase order and ask for the MTC to reference both. Dual certification with S35315 or TP310S is not possible because the chemistry windows conflict.
Hydrostatic test vs NDE — which do I get on S35045 pipe?
Each length is hydrotested or nondestructively electrically tested. Manufacturer may choose unless the purchase order fixes the method. If your piping class or client specification locks one method, state it on the PO and verify the chosen test appears on the MTC for every length—silent mill option is not the same as an approved project method.
What anneal temperature applies to UNS S35045?
Table 2 does not list S35045 individually, so the default 1900 °F [1040 °C] minimum with rapid cooling applies. Ask for that anneal temperature on the MTC and reject paperwork that copies a neighbouring grade’s higher practice without edition support.
What Table 1 chemistry defines UNS S35045?
Table 1 sets C 0.06–0.10%, Mn ≤1.50%, S ≤0.015%, Si ≤1.00%, Cr 25.0–29.0%, Ni 32.0–37.0%, Ti 0.15–0.60%, Cu ≤0.75%, and Al 0.15–0.60%; Mo, Nb, and N show as “…”. Phosphorus is also “…” in this pack’s extract—confirm in the purchaser’s edition. These are melting-analysis limits; order product analysis explicitly if receiving needs it.
What are the Table 4 tensile requirements for UNS S35045?
Table 4 requires 70 ksi [485 MPa] tensile and 25 ksi [170 MPa] yield minimum as a single row, with the standard 35% L / 25% T elongation pattern unless the ordered edition notes otherwise. Design to the code allowables listed for UNS S35045, not to a neighbouring 310 or S35315 strength line.
What filler metal should I use to weld UNS S35045 pipe?
Table 6 in the extracted edition assigns no AWS class to S35045, so filler is by agreement. Name the specific consumable on the WPS and PQR and qualify it on S35045 base metal before production welding. Mill WLD and HCW longitudinal welds are autogenous, so Table 6 applies only to fabrication joints with filler.
Is phosphorus limited for S35045?
In the Table 1 extract used for this pack, the phosphorus cell is an ellipsis (…)—no numeric maximum was captured. That is flagged as UNCERTAIN and should be confirmed against the purchaser’s ordered edition before receiving inspection treats a P value as a pass or fail. Do not invent a 0.045% or similar limit from neighbouring grades.

Conclusion

ASME SA312 UNS S35045 is a TP-less, high-Cr/Ni Ti+Al austenitic pipe grade with C 0.06–0.10%, Cr 25.0–29.0%, Ni 32.0–37.0%, Ti 0.15–0.60%, and Al 0.15–0.60%, a single 70/25 ksi Table 4 floor, and a default 1900 °F [1040 °C] Table 2 anneal. Table 6 assigns no filler class, so the consumable is by agreement. Phosphorus is listed as “…” in this pack’s extract—confirm in the purchaser’s edition. It is not a drop-in for ASME SA312 UNS S35315 Stainless Steel Pipe or ASME SA312 TP310S Stainless Steel Pipe. Order the manufacturing type, size and wall, finish, Ti/Al reporting, anneal proof, filler basis, and any product-analysis tests explicitly. For stock checks, mill certificates, or dual SA-312/A312 supply questions, contact SHH STEEL at admin@steelspecs.com or browse the ASME SA 312/SA 312M category on steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X