ASME SA312 UNS S20400 Stainless Steel Pipe | ASME SA312 Stainless Steel - SHH STEEL

ASME SA312 UNS S20400 Stainless Steel Pipe | SA 312/SA 312M

ASME SA312 UNS S20400 high-Mn nitrogen stainless steel pipe in SML, WLD and HCW, with Mn 7.0–9.0%, N 0.15–0.30% and Ni 1.50–3.00%, a 95/48 ksi Table 4 floor and a 1900 °F solution anneal, supplied by SHH STEEL to ASME B36.19 with EN 10204 3.1 MTCs.
Grade
UNS S20400
Standard
ASME SA312 / SA 312M (ASTM A312 / A312M)
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Dimensions
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA312 UNS S20400 Stainless Steel Pipe

ASME SA-312/SA-312M covers seamless, welded, and heavily cold-worked austenitic stainless steel pipe for high-temperature and general corrosive service. UNS S20400 is listed in Table 1 without a TP grade name — the grade column is printed as an ellipsis — so the material is identified on the purchase order, the stencil, and the certificate by its unified number alone. Commercially it may be called SA312 S20400 pipe, ASTM A312 S20400 pipe, or UNS S20400 stainless steel pipe, and the order should always say “UNS S20400” plus the edition of the standard rather than a market nickname.

S20400 is a high-manganese, nitrogen-alloyed austenitic grade with very lean nickel. Table 1 sets C ≤0.030%, Mn 7.0–9.0%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 15.0–17.0%, Ni 1.50–3.00%, and N 0.15–0.30%, with no molybdenum or copper requirement. The manganese and nitrogen do the work that nickel does in 18-8 grades, and they give a strong pipe: Table 4 sets 95 ksi tensile and 48 ksi [330 MPa] yield minimum, with the tensile SI value printed as 635 MPa in the standard. The pipe is solution annealed at the Table 2 default of 1900 °F [1040 °C] minimum, and Table 6 lists ER209 as the filler.

SHH STEEL can supply ASME SA312 UNS S20400 stainless steel pipe to the edition named on your enquiry, in seamless (SML), welded (WLD), and heavily cold-worked (HCW) form. We quote ASME B36.19 schedules and special OD and wall by agreement, ship with EN 10204 3.1 mill test certificates that report the full Table 1 chemistry including manganese and nitrogen, and offer dual SA-312/A312 marking when the heat and tests meet both editions on the purchase order. Please confirm NPS, wall or schedule, finish, length practice, and any supplementary tests when you enquire.

The names below are the ones buyers commonly use, and they map to the ordered product as shown. Because there is no TP name, the UNS number is the only reliable identity on paper.

  • ASME SA312 UNS S20400 — preferred marking language for ASME-code and dual-marked pipe
  • ASTM A312 S20400 — same grade tables when the ASTM edition is referenced
  • “S20400” or “204” pipe — market shorthand; confirm SA-312/A312 and the Table 1 limits on the order
  • EN / JIS names — high-Mn nitrogen grades vary by region, so treat any map as approximate only

Sister grades buyers compare with S20400 include ASME SA312 TP201 Stainless Steel Pipe (Mn 5.5–7.5%, Ni 3.5–5.5%, 75/38 ksi), ASME SA312 TP201LN Stainless Steel Pipe (low carbon, Ni 4.0–5.0%, 95/45 ksi), ASME SA312 TPXM-19 Stainless Steel Pipe on the high-strength nitrogen side, and ASME SA312 TP304L Stainless Steel Pipe or ASME SA312 TP316L Stainless Steel Pipe when corrosion matters more than strength. Grade hub: ASME SA 312/SA 312M.

Manufacturing Types (SML / WLD / HCW)

ASME SA-312 recognizes three manufacturing routes for UNS S20400 pipe, and the route is a purchase-order decision driven by the design code, the size range, wall thickness, and how the owner wants the pipe inspected. The route never changes the chemistry: whichever way the pipe is made, the heat must still meet C ≤0.030%, Mn 7.0–9.0%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 15.0–17.0%, Ni 1.50–3.00%, and N 0.15–0.30%, and every length must still go through the solution anneal at 1900 °F [1040 °C] minimum before it is released.

  • Seamless (SML) — no welding at any stage. Seamless is used for heavier walls and smaller bores, but many S20400 orders are welded from strip, and every length still receives the 1900 °F solution anneal before release.
  • Welded (WLD) — automatic welding without filler metal, with the weld finished so the pipe meets dimensional and mechanical requirements after the final heat treatment. The strip or plate heat must itself carry the full UNS S20400 chemistry, so ask for the coil or plate heat number on the certificate.
  • Heavily cold-worked (HCW) — welded pipe cold worked to at least 35% reduction of wall and weld before the final anneal, again without filler in the longitudinal seam, with the weld radiographed before cold work. Order HCW when the project specifically wants that marking and the process controls SA-312 writes around it.

Every finished length is hydrostatically tested or nondestructively electrically tested, and the mill may choose the method unless the purchase order fixes one. Pipe NPS 10 and larger may ship marked “NH” only when the purchaser accepts a system test in place of the hydrotest, and lots for mechanical testing follow clause 11.1. S20400 carries no H-grade lot-marking or grain-size rule, but heat identity and the UNS number must be stenciled on every length, because there is no TP name to fall back on.

UNS S20400 is a niche grade in SA-312 pipe, so most orders are mill runs rather than stock. Strip chemistry must meet the full S20400 row, including the high manganese and nitrogen, so ask for the coil heat number and confirm the edition year, route, sizes, and wall on enquiry so the mill can plan the heat from the start.

Chemical Composition of SA312 UNS S20400

Two chemistry layers matter for UNS S20400. The melting (heat or ladle) analysis is mandatory for every heat under SA-312/A312 Table 1, while product analysis on finished pipe applies only when it is ordered through Supplementary Requirement S1 or purchase-order wording. Product tolerances are not printed in SA-312 itself; they come through ASTM A999/A999M §6.3 from ASTM A480/A480M Table A1.1. SHH STEEL reports the actual ladle values and, when ordered, the product values, and never quotes tighter catalogue windows that the standard does not publish.

Melting analysis (heat / ladle analysis) — Table 1

The table below is the heat analysis for UNS S20400 from SA-312/SA-312M Table 1. Values are maximum unless a range is shown, and an ellipsis (…) means the ordered edition sets no requirement for that element. S20400 has no molybdenum or copper requirement in Table 1, and there is no TP letter for this UNS.

Element UNS S20400 melting analysis
Carbon (C) ≤ 0.030
Manganese (Mn) 7.0 – 9.0
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.030
Silicon (Si) ≤ 1.00
Chromium (Cr) 15.0 – 17.0
Nickel (Ni) 1.50 – 3.00
Nitrogen (N) 0.15 – 0.30
Molybdenum (Mo) … (no requirement)
Copper (Cu) … (no requirement)

Product analysis — A480/A480M Table A1.1 tolerances applied to Table 1

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) ≤ 0.030 0.005 over ≤ 0.035
Manganese (Mn) 7.0 – 9.0 0.06 under / over 6.94 – 9.06
Phosphorus (P) ≤ 0.045 0.010 over ≤ 0.055
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) ≤ 1.00 0.05 over ≤ 1.05
Chromium (Cr) 15.0 – 17.0 0.20 under / over 14.80 – 17.20
Nickel (Ni) 1.50 – 3.00 0.07 under / over 1.43 – 3.07
Nitrogen (N) 0.15 – 0.30 0.01 under / 0.03 over 0.14 – 0.33

Source: SA-312 Table 1 UNS S20400 (grade column “…”). N 0.15–0.30% required; no Mo or Cu requirement.

Manganese at 7.0–9.0% and nitrogen at 0.15–0.30%, combined with only 1.50–3.00% nickel, are what separate S20400 from ASME SA312 TP201 Stainless Steel Pipe (Mn 5.5–7.5%, Ni 3.5–5.5%, N ≤0.25% maximum) and ASME SA312 TP201LN Stainless Steel Pipe (Mn 6.4–7.5%, Ni 4.0–5.0%, N 0.10–0.25%, Cu ≤1.00%). Carbon at ≤0.030% is in the low-carbon band, and chromium at 15.0–17.0% is lower than the 18.0–20.0% of ASME SA312 TP304 Stainless Steel Pipe, which is why the grade should not be treated as a drop-in for 18-8 pipe.

When product analysis is ordered, A480 Table A1.1 widens the Table 1 limits as shown above: carbon up to 0.035%, Mn 6.94–9.06%, Si up to 1.05%, Cr 14.80–17.20%, Ni 1.43–3.07%, and N 0.14–0.33%. These are acceptance limits for finished pipe, not melt targets, and nitrogen should always be reported because it carries much of the strength.

Mechanical Properties of SA312 UNS S20400

Room-temperature tensile requirements for UNS S20400 come from SA-312 Table 4 and are summarized below. These are minimum release values for the lot, not typical values, and design allowables must always be taken from the governing code tables for UNS S20400 rather than from a neighbouring grade.

Property UNS S20400 requirement (Table 4)
Tensile strength, min 95 ksi [635 MPa]
Yield strength (0.2% offset), min 48 ksi [330 MPa]
Elongation in 2 in. or 50 mm (or 4D) 35% longitudinal / 25% transverse, min

The 95/48 ksi floors put S20400 at the top of the lean-nickel group: it shares the 95 ksi tensile band with ASME SA312 TP201LN Stainless Steel Pipe but has a higher 48 ksi yield, and both are far above the 75/38 ksi of ASME SA312 TP201 Stainless Steel Pipe and the 75/30 ksi of ASME SA312 TP304 Stainless Steel Pipe and ASME SA312 TP316 Stainless Steel Pipe. Note that Table 4 prints 635 MPa as the SI tensile value for this UNS rather than the 655 MPa used for other 95 ksi rows; we quote it as published. Table 4 does not list a hardness maximum for S20400.

Design should use Table 4 and the code allowable stresses for UNS S20400 where the design code accepts the grade, not values borrowed from TP201 or TP304, unless the mill has accepted higher guaranteed values in writing. Tension and flattening or bend tests run on a lot basis, supplementary tests apply only when listed on the order, and delivery is always the solution-annealed condition.

Dimensions and Tolerances

Dimensional supply for SA312 UNS S20400 pipe follows ASME B36.19 schedules for the common NPS and schedule combinations, with special OD and wall available by agreement when a project needs a section the schedules do not cover. Outside-diameter variations follow ASTM A999/A999M, and wall-thickness variations follow SA-312 Table 3 as summarized below. State on the purchase order whether wall is nominal or minimum (Supplementary S8), because the two readings produce different pipe from the same size line.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

Source: SA-312 Table 3; outside diameter variations per A999/A999M.

  • Lengths — single random, double random, or cut-to-length on order
  • Cut lengths — typically no more than 1/4 in. [6 mm] over the ordered length unless the PO states a tighter band
  • Ends — plain or beveled; confirm bevel angle and root face when the WPS is already frozen

Many utility, structural, and general process buyers order by OD × wall rather than NPS and schedule, which is fine as long as the enquiry says so clearly. Straightness, end finish, and length tolerance should be written into export orders so receiving inspection has an agreed acceptance basis instead of arguing after arrival. On thin schedules with threaded or socket-weld ends, check that the remaining wall is still adequate after the 12.5% under-tolerance. Jointers are not permitted unless the purchase order allows them, so cut-to-length programmes should include an allowance for fit-up scrap rather than expecting the mill to ship short pieces.

Equivalent Grades

UNS S20400 has a close equivalent in ASTM A312, but there is no single EN or JIS grade that maps one-to-one. Regional high-manganese nitrogen designations help material selection, and none of them is an automatic substitute for ASME pressure-code pipe without an approved material specification and design-code acceptance.

Designation Notes
ASME SA-312 / ASTM A312 UNS S20400 Governing pipe product standard for this article (no TP letter in Table 1)
UNS S20400 Unified number listed in Table 1
EN / JIS approximations High-Mn N-alloyed austenitic names vary by region; confirm the applicable EN or JIS product specification when ordering non-ASME product—do not mark EN/JIS alone on an SA-312 MTC
Related plate (201 family) ASME SA240 UNS S20100 Stainless Steel Plate — neighboring Mn–N plate UNS; not S20400

The 201-family flat product commonly offered is S20100 plate, which is a neighbouring Mn–N UNS and not S20400, so confirm the plate UNS on any matching plate order. Within SA-312, S20400 must not be interchanged with ASME SA312 TP201 Stainless Steel Pipe (S20100) or ASME SA312 TP201LN Stainless Steel Pipe (S20153), because each has its own Table 1 and Table 4 rows. Related SA-312 pages: ASME SA312 TP201 Stainless Steel Pipe, ASME SA312 TP201LN Stainless Steel Pipe, ASME SA312 TPXM-19 Stainless Steel Pipe, and ASME SA312 TP304L Stainless Steel Pipe.

Heat Treatment and Delivery Condition

S20400 has no individual row in Table 2, so it falls under the default for all grades not individually listed: solution anneal at 1900 °F [1040 °C] minimum, followed by water quenching or another rapid cool fast enough to prevent harmful carbide reprecipitation. Seamless pipe may be quenched directly after hot forming where the edition allows and the finishing temperature is not below the minimum anneal temperature. HCW product is cold reduced before the final anneal, so cold work is never the delivery condition.

SHH STEEL ships S20400 solution annealed and pickled, or bright annealed by agreement, straightened, cut to the ordered length practice, and hydrotested or electrically tested per length. The high manganese and nitrogen make the grade work harden quickly, so heavy cold bending after delivery may need a fresh solution anneal to restore ductility. The anneal temperature and cooling method should appear on the certificate.

Corrosion Resistance

SA-312 does not contain a corrosion table, so this section is engineering commentary. With 15.0–17.0% chromium, no molybdenum, and very lean nickel, S20400 is generally a little below ASME SA312 TP304L Stainless Steel Pipe in general and pitting resistance, and it is chosen for strength, galling resistance, and nickel economy rather than for aggressive corrosion. The low carbon helps welded joints resist intergranular attack, and nitrogen gives a modest pitting benefit.

  • Atmospheric and mild water service — generally suitable in clean indoor or mild outdoor conditions
  • Chlorides — less resistant than molybdenum grades; prefer ASME SA312 TP316 Stainless Steel Pipe or ASME SA312 TP316L Stainless Steel Pipe in chloride-bearing or coastal duty
  • Intergranular corrosion — low risk as-welded thanks to C ≤0.030%; S7 (A262 Practice E) available when proof is needed
  • Chloride stress corrosion cracking — similar susceptibility to other austenitic grades

Confirm the fluid, chloride level, and temperature before selecting S20400, and treat it as a strength and cost choice rather than a corrosion upgrade from TP304.

Applications of SA312 UNS S20400 Pipe

Applications for UNS S20400 pipe are driven by its high Table 4 strength and lean-nickel chemistry, in services where 304-class corrosion resistance is adequate. The table below summarizes where buyers typically specify it.

Application area Typical use of S20400 pipe Selection note
Utility and process piping Water, air, mild chemical transfer lines ordered to SA-312 Confirm fluid compatibility with S20400 chemistry
Structural / architectural Handrail, support, and decorative pipe ordered as SA-312 product 48 ksi min yield can help section design vs TP304
Transportation / OEM Frames and piping kits converting to SA-312 documentation Dual SA312/A312 marking often requested; mark UNS S20400 clearly
General corrosive service Mild to moderate environments without heavy chlorides Prefer TP316/TP316L if chlorides dominate
High-strength lean-nickel service Where 95/48 ksi Table 4 floors are specified with S20400 chemistry Do not substitute TP201 or TP201LN without engineering review
Cost-sensitive austenitic piping Where lean Ni bill of material is accepted by the end-user Fitness for service first; nickel savings second

Typical users include utility and low-pressure process piping, structural and mechanical tube, and general service with mild fluids where the design code accepts S20400. Enquiries should state the process fluid and temperature, the code acceptance of S20400, and any S7 corrosion test. When the fluid is more aggressive, ASME SA312 TP304L Stainless Steel Pipe or ASME SA312 TP316L Stainless Steel Pipe are usually safer, and when a TP grade name is mandatory on the drawing, compare with ASME SA312 TP201LN Stainless Steel Pipe.

Weldability

S20400 welds by GTAW, GMAW, SMAW, and orbital processes with normal austenitic practice: clean joints, controlled heat input and interpass temperature, and back-purged roots. Procedures should be qualified on the actual high-Mn, lean-nickel chemistry. SA-312 Table 6 lists ER209 (UNS S20980 / W32240) as the recommended filler for S20400 when mill seam repairs use filler metal under Section 15, and ER209 is also the usual matching high-Mn nitrogen consumable for field girth welds.

  • ER209 on the WPS/PQR — matches the strength and nitrogen of the base metal
  • Do not assume ER308 — it is not the Table 6 filler for this UNS and may undermatch strength
  • GTAW roots — preferred for thin walls and clean ID profiles
  • Back-purge — argon or equivalent to protect the ID from heat tint

Record the agreed AWS or EN consumable on the welding procedure so the weld meets the 95/48 ksi base-metal strength where the design relies on it. Mill longitudinal welds on WLD and HCW pipe are made without filler, so Table 6 applies to repair and fabrication joints only, and girth-weld NDE follows the fabrication code.

Surface Finishes

Surface condition for SA312 UNS S20400 pipe should be stated on the purchase order rather than left to mill default. For stainless pipe, embedded free iron, residual scale, and chloride-bearing residues are where corrosion starts, so the finish is part of the material performance and not just appearance. The finishes we regularly quote for this grade are listed below.

  • Annealed and pickled (AP) — solution annealed at 1900 °F [1040 °C] minimum, then descaled in acid pickle or an equivalent process to a matte grey finish; the standard choice for process pipe
  • Blasted and pickled — common on heavy-wall seamless where blasting first makes scale removal more reliable
  • Bright annealed (BA) — annealed in a protective atmosphere where mill capability exists for the size; the anneal temperature still has to meet the Table 2 practice for UNS S20400
  • Mechanically polished — OD and/or ID polish to an agreed grit or Ra when ordered; polishing never replaces the solution anneal
  • Bead-finished welded OD — weld bead rolled or ground flush as agreed on WLD and HCW product

For S20400 the usual choice is annealed and pickled, with bright annealed finishes available by agreement on smaller sizes. Passivation after pickling or polishing can be added when the end-user specification calls for it, even though SA-312 itself does not require it. If the project bans chloride-bearing marking inks, say so on the order; otherwise the mill will apply its normal stencil practice and ship its default AP finish.

Inspection and Testing

The base acceptance package for SA-312 UNS S20400 pipe combines chemistry, tensile testing, heat-treatment evidence, and a pressure or electrical integrity test on every length. The items below make up the usual package; supplementary requirements and project corrosion tests only apply when they are written on the purchase order.

  • Heat (melting) analysis — mandatory per heat against Table 1 for UNS S20400: C ≤0.030%, Mn 7.0–9.0%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 15.0–17.0%, Ni 1.50–3.00%, and N 0.15–0.30%
  • Product analysis — when ordered (Suppl. S1 or PO wording), using A480 Table A1.1 tolerances via A999 §6.3
  • Tension test — 95 ksi [635 MPa as printed] tensile and 48 ksi [330 MPa] yield minimum, with 35% longitudinal / 25% transverse elongation on a lot basis
  • Flattening test — or the alternate bend test where the standard permits
  • Hydrostatic or nondestructive electric test — every length; manufacturer’s option unless the order fixes the method
  • Visual and dimensional check — against ordered NPS/schedule or OD × wall, with UNS S20400 on every stencil

Mill test certificates: EN 10204 3.1 is the standard documentation from SHH STEEL supply. For S20400 the certificate must report the full Table 1 chemistry including Mn 7.0–9.0% and N 0.15–0.30%, the 95/48 ksi tensile results and 35%/25% elongation, the hydro or NDE method, and the 1900 °F anneal. EN 10204 3.2 or third-party witness by SGS, Bureau Veritas, TÜV, or the buyer’s nominated agency is arranged when specified, and it should be booked before final testing rather than after the heat has been released. Dual ASME SA-312 / ASTM A312 certification is available when chemistry, heat treatment, mechanical tests, and marking satisfy both editions named on the order.

Option Purpose
S1 product analysis Confirms chemistry on finished pipe
S5 radiography Weld integrity on WLD pipe
S7 intergranular corrosion A262 Practice E after sensitizing treatment
S8 minimum wall Wall interpreted as minimum rather than nominal
S9 weld decay Compares weld and base-metal loss rates

Receiving review should confirm C ≤0.030%, Mn 7.0–9.0%, Cr 15.0–17.0%, Ni 1.50–3.00%, N 0.15–0.30%, the 95/48 ksi tensile results, elongation, and the anneal statement. Check that the stencil reads UNS S20400 and not TP201 or TP201LN, and use the certificate rather than a PMI gun to confirm nitrogen.

Packaging and Shipping

Export and domestic shipments of SA312 UNS S20400 pipe are packed for handling and for ocean or land transport. The packing we normally apply is summarized below, and anything beyond it can be agreed on the order.

  • Seaworthy bundles — pipes strapped or cradled in bundles sized for container or break-bulk handling, with non-metallic separators where the finish needs protecting
  • End caps — plastic or metal caps on plain or beveled ends to keep out damage and contamination in transit
  • Marking — specification, grade (UNS S20400), heat number, size, manufacturing type (SML / WLD / HCW), test letters, and mill identity as SA-312 and the purchase order require
  • Export protection — waterproof wrapping or desiccant as agreed for polished or bright-annealed finishes, with low-chloride inks on request

Segregate S20400 from ASME SA312 TP201 Stainless Steel Pipe, ASME SA312 TP201LN Stainless Steel Pipe, and 300-series stock on the packing list and in the yard, because they look identical. Use separate bundles and distinct tags on mixed shipments, and have receiving inspectors check stencil heat numbers and the UNS against the MTC for every length. Keep interiors dry and capped so chloride-bearing moisture cannot stain or pit the surface before installation. Shipping documents normally include the packing list, invoice, bill of lading or air waybill, and the 3.1 or 3.2 MTC with full Table 1 chemistry, plus origin and customs papers to suit the agreed Incoterms.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless plate and pipe, and for SA312 UNS S20400 we quote against the edition you name rather than a generic catalogue sheet. We report the full Table 1 chemistry on the MTC including manganese and nitrogen, together with the 95/48 ksi results and the 1900 °F anneal statement, so the S20400 identity is clear on paper even without a TP name. Heat identity stays unbroken from the melt to the finished length, so receiving inspection can clear each heat against Table 1 and Table 4 without chasing paperwork after the pipe has arrived.

We check supplier certificates before shipment for 201-family stock relabelled as S20400, nitrogen below 0.15%, or nickel outside the 1.50–3.00% window, so problems are caught at the mill rather than at the fabricator. Where a project mixes lean-nickel and 300-series pipe, we keep heats and paperwork separate from the start.

  • Specification fidelity — chemistry and tensile to SA-312/A312 Table 1 and Table 4 for UNS S20400; Mn and N reported; 1900 °F anneal stated; heat number and UNS on every length
  • Mill resources — SML, WLD, and HCW from qualified stainless pipe mills with heat traceability; cutting and beveling on confirmed orders
  • Documentation — EN 10204 3.1 MTCs as standard with full Table 1 chemistry; 3.2 or third-party inspection on request
  • Dual marking — ASME SA-312 and ASTM A312 when the heat and tests meet both editions you name
  • Related grades — ASME SA312 TP201 Stainless Steel Pipe, ASME SA312 TP201LN Stainless Steel Pipe, ASME SA312 TP304L Stainless Steel Pipe, and ASME SA312 TP316L Stainless Steel Pipe when a project buys a matched package
  • Export packing — seaworthy bundles, end protectors, and durable grade, heat, size, and type marking

Quotations follow your purchase-order language for edition year, manufacturing type, size, wall, finish, and any supplementary tests you name (S1, S5, S7, S8, S9). If the same project also needs plate or fittings, ask for coordinated heats so the chemistry lines up across product forms. Grade hub: ASME SA 312/SA 312M.

Supply Capability

SHH STEEL can supply ASME SA312 UNS S20400 stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade.

Item SHH STEEL capability for UNS S20400
Standard ASME SA-312/SA-312M and/or ASTM A312/A312M UNS S20400 (no TP designation in Table 1)
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD/wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length SRL, DRL, or cut-to-length
Finish Annealed and pickled; blasted and pickled; bright annealed or polished by agreement
Testing Tension (95/48 ksi), flattening/bend, hydro or NDE per length; full Table 1 chemistry with Mn and N on MTC; 1900 °F anneal stated; S1/S5/S7/S8/S9 on order
Documents EN 10204 3.1 with full Table 1 chemistry; third-party inspection / 3.2 on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

UNS S20400 is rarely held in stock as SA-312 pipe, so most orders are mill runs; small quantities can sometimes be grouped with other lean-nickel production. We check any stock certificate against the S20400 row before offering it. Enquiries should state the SA-312 edition, UNS S20400, SML/WLD/HCW, NPS or OD × wall (and whether wall is nominal or minimum), length practice, finish, and any product-analysis, corrosion-test, or 3.2 requirements, so mill slots line up with your need date. Cut lengths, beveling, and packing-list marking are available on confirmed orders, and grouping project sizes onto one heat keeps the chemistry consistent while helping meet mill minimums without over-ordering.

FAQ

Is ASME SA312 the same as ASTM A312 for UNS S20400?
For chemistry (Table 1), tensile requirements (Table 4), manufacturing types, and most testing language, ASME SA-312/SA-312M follows ASTM A312/A312M of the edition it references, so the grade rows for UNS S20400 / UNS S20400 read the same. Dual SA-312/A312 marking is common and we supply it when the heat and the tests satisfy both editions named on the purchase order.
Why does UNS S20400 have no TP grade name?
In SA-312 Table 1 the grade column for S20400 is printed as an ellipsis, so the material is identified only by its unified number. Write “UNS S20400” on the purchase order, the stencil, and the certificate, and do not let anyone substitute a TP201 or TP201LN label, because those are different UNS numbers with different chemistry and tensile rows.
Seamless vs welded UNS S20400 — which should I order?
Neither route is better in every case. Seamless is the usual choice for heavy walls, high pressure, and small bores where the owner prefers no longitudinal seam, while welded pipe is economical in thinner walls and larger diameters and is made without filler metal. Both must meet the same Table 1 chemistry, the same 95/48 ksi Table 4 floor, and the same solution anneal, so let the design code and the size range decide.
Hydrostatic test or NDE — which will my UNS S20400 pipe get?
Every length must pass either a hydrostatic test or a nondestructive electric test, and SA-312 leaves the choice to the manufacturer unless the purchase order fixes the method. If your inspection plan or the owner’s specification needs a hydrotest on every length, or a particular eddy-current or ultrasonic practice, write it on the order so the mill plans for it before production starts.
Does SA-312 Table 4 set a hardness limit for UNS S20400?
No. Table 4 gives the tensile strength, yield strength, and elongation minima for UNS S20400, but it does not list a hardness maximum. Catalogue Brinell or Rockwell figures you may see elsewhere are typical values, not specification requirements. If hardness matters for your fabrication or for the end user, state the limit on the purchase order and we will make sure it is tested and reported on the certificate.
What filler metal should I use to weld UNS S20400 pipe?
SA-312 Table 6 lists ER209 (UNS S20980 / W32240) as the recommended filler for UNS S20400 when filler is used on mill seam repairs, and ER209 is also the usual consumable for field girth welds. It matches the high-manganese nitrogen chemistry and the strength of the pipe. Record the classification on the WPS and PQR, and do not substitute ER308 without engineering review.
What wall-thickness tolerance applies to UNS S20400 pipe?
Wall tolerance follows SA-312 Table 3: 12.5% under for every size band, with the over-tolerance ranging from 15.0% to 22.5% depending on NPS, t/D ratio, and whether the pipe is seamless or welded. If your design is based on minimum wall rather than nominal wall, order Supplementary Requirement S8 so the mill rolls to the right target from the start.
Which sister grades do buyers compare with UNS S20400?
Buyers most often compare S20400 with ASME SA312 TP201 Stainless Steel Pipe on cost, ASME SA312 TP201LN Stainless Steel Pipe when a TP grade name is required, ASME SA312 TPXM-19 Stainless Steel Pipe for high-strength nitrogen service, and ASME SA312 TP304L Stainless Steel Pipe or ASME SA312 TP316L Stainless Steel Pipe where corrosion matters more than strength. Each has its own Table 1 and Table 4 rows, so check the design basis and code allowables before substituting one for another.
UNS S20400 vs TP201LN — what is the difference?
S20400 has higher manganese (7.0–9.0% vs 6.4–7.5%), higher nitrogen (0.15–0.30% vs 0.10–0.25%), much leaner nickel (1.50–3.00% vs 4.0–5.0%), lower chromium (15.0–17.0% vs 16.0–17.5%), and no copper limit. Both have a 95 ksi tensile floor, but S20400 carries a 48 ksi yield against 45 ksi. They are separate Table 1 rows and must not be interchanged.
Why does Table 4 show 635 MPa for S20400?
SA-312 Table 4 prints the 95 ksi tensile minimum for UNS S20400 with an SI value of 635 MPa, rather than the 655 MPa used on other 95 ksi rows such as TP201LN. We quote the figure exactly as published in the ordered edition. If your project works in SI units, confirm on the purchase order which value governs acceptance so there is no dispute.
What heat treatment does SA-312 require for S20400?
S20400 falls under the Table 2 default for grades not individually listed: solution anneal at 1900 °F [1040 °C] minimum, then water quench or another rapid cool that prevents carbide reprecipitation. Delivery is always the annealed condition, including HCW pipe, and the certificate should state the anneal temperature and cooling method so receiving inspection can confirm Table 2 was met.
What product-analysis limits apply to UNS S20400?
Product analysis applies only when ordered through Supplementary Requirement S1 or purchase-order wording. A480 Table A1.1 tolerances, via A999 §6.3, give C ≤0.035%, Mn 6.94–9.06%, P ≤0.055%, S ≤0.035%, Si ≤1.05%, Cr 14.80–17.20%, Ni 1.43–3.07%, and N 0.14–0.33%. These are finished-pipe acceptance limits, not targets for the melt.

Conclusion

ASME SA312 UNS S20400 is the high-manganese, nitrogen-alloyed, lean-nickel pipe grade in SA-312, identified by UNS only, with C ≤0.030%, Mn 7.0–9.0%, Cr 15.0–17.0%, Ni 1.50–3.00%, and N 0.15–0.30%, a 95/48 ksi Table 4 floor (635 MPa tensile as printed) with 35% L / 25% T elongation, a 1900 °F [1040 °C] solution anneal, and ER209 filler from Table 6. It is not interchangeable with ASME SA312 TP201 Stainless Steel Pipe or ASME SA312 TP201LN Stainless Steel Pipe. Order the UNS, manufacturing type, size and wall, finish, and supplementary tests explicitly. For stock checks, mill certificates, or dual SA-312/A312 supply questions, contact SHH STEEL at admin@steelspecs.com or browse the ASME SA 312/SA 312M category on steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X