ASME SA312 TP347LN Stainless Steel Pipe | ASME SA312 Stainless Steel - SHH STEEL

ASME SA312 TP347LN Stainless Steel Pipe | SA 312/SA 312M

ASME SA312 TP347LN (UNS S34751) stainless steel pipe under SA-312/SA-312M (ASTM A312/A312M): seamless (SML), welded (WLD) and heavily cold-worked (HCW); C 0.005–0.020%, N 0.06–0.10%, Nb 0.20–0.50% (≥15×C); Table 4 minima 75/30 ksi; solution annealed. SHH STEEL supplies with EN 10204 3.1 MTCs.
Grade
TP347LN / UNS S34751
Standard
ASME SA312 / SA 312M (ASTM A312 / A312M)
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA312 TP347LN Stainless Steel Pipe

ASME SA-312/SA-312M covers seamless, welded, and heavily cold-worked austenitic stainless steel pipe intended for high-temperature and general corrosive service. Grade TP347LN is listed in Table 1 as UNS S34751. Commercially the same product may be called SA312 TP347LN pipe, ASTM A312 TP347LN pipe, A312 Grade TP347LN, or 347LN stainless steel pipe when the purchase order clearly references SA-312 or A312. For pressure piping and code work, cite the full grade designation, the UNS number, and the edition of the standard on the purchase order and on the mill test certificate—do not rely on a bare “347LN” market label.

TP347LN is a low-carbon, nitrogen-bearing, niobium-stabilized austenitic grade—the LN companion to classic ASME SA312 TP347 Stainless Steel Pipe. Table 1 locks carbon at 0.005–0.020%, requires nitrogen at 0.06–0.10%, and sets niobium at 0.20–0.50% with footnote I requiring Nb not less than 15 times the carbon content. Chromium remains in the 17.0–19.0% band and nickel in the 9.0–13.0% band; molybdenum is not required. That chemistry supports the Table 4 tensile floor of 75 ksi min / 30 ksi min yield while keeping carbon very low for welded service. It is not an H grade: Table 2 uses the default solution-annealing temperature of 1900 °F [1040 °C], Table 6 filler guidance follows the ER347 family, and supplementary requirement S6 (stabilization) applies only when the purchase order specifies it.

SHH STEEL can supply ASME SA312 TP347LN stainless steel pipe to the edition named on the enquiry, including seamless (SML), welded (WLD), and heavily cold-worked (HCW) routes; ASME B36.19 schedules and special OD/wall by agreement; EN 10204 3.1 mill test certificates; and dual SA-312/A312 marking when the heat analysis, heat treatment, mechanical tests, and marking satisfy both editions named on the purchase order. Confirm NPS, wall or schedule, finish, length practice, and any product-analysis or supplementary tests on enquiry.

Common commercial names and how they map to the ordered product are listed below—use the full SA-312/A312 designation on the purchase order rather than market shorthand alone.

  • ASME SA312 TP347LN / SA-312 Grade TP347LN — preferred marking language for ASME-code and dual-marked pipe
  • ASTM A312 TP347LN — same grade tables for chemistry and tensile when the ASTM edition is referenced
  • UNS S34751 — unified numbering system identity used on MTCs and in cross-reference tables
  • 347LN stainless steel pipe — market shorthand; confirm the LN carbon, nitrogen, and Nb ≥15×C rules on the order

TP347LN is not “347 with a little nitrogen.” Heats that only meet TP347 footnote G (Nb ≥10×C / 1.00% max) without the LN carbon, nitrogen, and Nb range are not TP347LN. UNS S34751 must appear with the TP name on stencil and MTC. Related grades: ASME SA312 TP347 Stainless Steel Pipe, ASME SA312 TP347H Stainless Steel Pipe, ASME SA312 TP316LN Stainless Steel Pipe. Hub: ASME SA 312/SA 312M.

Manufacturing Types (SML / WLD / HCW)

ASME SA-312 defines three manufacturing routes that may be marked on finished TP347LN pipe. Selecting the route is a purchase-order decision driven by design code, size range, wall thickness, and inspection preference. It does not change the Table 1 chemistry of Grade TP347LN—melting must still meet C 0.005–0.020%, N 0.06–0.10%, Nb 0.20–0.50%, and Nb ≥15×C.

  • Seamless (SML) — no welding at any stage of manufacture. Seamless is preferred when the project specification excludes welded pipe, when thick walls favor seamless production, or when the piping class documentation is written around seamless product only.
  • Welded (WLD) — automatic welding without filler metal. The weld is finished so that the pipe meets dimensional and mechanical requirements after the final heat treatment required by SA-312. Welded product is widely used for common NPS and schedule combinations where the code accepts welded austenitic pipe.
  • Heavily cold-worked (HCW) — welded pipe that is cold worked to a reduction of area of wall and weld of at least 35% before the final anneal, again without filler metal in the longitudinal weld. HCW is ordered when the buyer wants the HCW marking and the process controls written into SA-312 for that route.

Each finished length is hydrostatically tested or nondestructively electrically tested. The manufacturer may choose the method unless the purchase order fixes one. Marking on the pipe typically includes the manufacturer, grade (TP347LN), heat number, NPS or outside diameter and schedule or wall thickness, and the manufacturing type letters SML, WLD, or HCW. When comparing seamless versus welded TP347LN offers, check manufacturing type and the hydro or NDE method on the mill test certificate—not only the grade stamp.

Chemical Composition of SA312 TP347LN

Two chemistry layers matter: melting (heat / ladle) analysis—mandatory per heat under ASME SA-312/ASTM A312 Table 1—and product analysis when ordered (Suppl. S1 / PO). SA-312/A312 defer product-analysis tolerances through ASTM A999/A999M §6.3 to ASTM A480/A480M Table A1.1. SHH STEEL reports actual ladle and, when ordered, product values—never unpublished tighter windows.

Melting analysis (heat / ladle analysis) — Table 1

Heat analysis for Grade TP347LN / UNS S34751 from ASME SA-312/SA-312M (ASTM A312/A312M) Table 1 is summarized below. Values are maximum unless a range is shown; ellipses (…) mean no requirement in the ordered edition.

Element TP347LN / UNS S34751 melting analysis
Carbon (C) 0.005 – 0.020
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.030
Silicon (Si) ≤ 1.00
Chromium (Cr) 17.0 – 19.0
Nickel (Ni) 9.0 – 13.0
Molybdenum (Mo) No requirement (…)
Niobium (Nb) 0.20 – 0.50 (and ≥ 15 × C per footnote I)
Nitrogen (N) 0.06 – 0.10

Source: ASME SA-312/SA-312M ≡ ASTM A312/A312M Table 1 for Grade TP347LN, including footnote I (Nb ≥15×C for S34751). Do not treat secondary catalog sheets as a substitute for the ordered edition.

The LN carbon band is far tighter than TP347’s ≤0.08% ceiling, nitrogen is mandatory, and niobium must satisfy both the 0.20–0.50% window and footnote I’s 15×C minimum. Example: at C = 0.015%, 15×C = 0.225%, so Nb must be ≥0.225% and ≤0.50%. At C = 0.020%, 15×C = 0.30%.

Product analysis — A480/A480M Table A1.1 tolerances applied to Table 1

When product analysis is ordered, finished-pipe chemistry shall meet Table 1 as modified by the product-analysis tolerances of ASTM A480/A480M Table A1.1 (via A999 §6.3). The verified product-analysis limits for TP347LN are:

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) 0.005 – 0.020 0.005 under / over 0.000 – 0.025
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.045 0.010 over ≤ 0.055
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) ≤ 1.00 0.05 over ≤ 1.05
Chromium (Cr) 17.0 – 19.0 0.20 under / over 16.80 – 19.20
Nickel (Ni) 9.0 – 13.0 0.10 under / 0.15 over 8.90 – 13.15
Niobium (Nb) 0.20 – 0.50 0.05 under / over 0.15 – 0.55
Nitrogen (N) 0.06 – 0.10 0.01 under / over 0.05 – 0.11

Versus TP347: much lower carbon band, intentional nitrogen, and Nb as a fixed range plus 15×C—not footnote G’s 10×C / 1.00% max alone. Versus TP316LN: Nb stabilization instead of molybdenum 2–3%; do not treat the two LN grades as interchangeable when chloride pitting dominates. If an enquiry only says “347LN stainless pipe,” confirm Table 1 limits, manufacturing type, and whether product analysis is required before rolling.

Mechanical Properties of SA312 TP347LN

Tensile requirements for TP347LN are given in ASME SA-312/SA-312M (ASTM A312/A312M) Table 4. Specimens and orientation follow the testing clauses of the standard and the referenced general requirements (A999/A999M as applicable).

Property TP347LN requirement (Table 4)
Tensile strength, min 75 ksi [515 MPa]
Yield strength (0.2% offset), min 30 ksi [205 MPa]
Elongation in 2 in. or 50 mm (or 4D) 35% longitudinal / 25% transverse, min

These minima are the mandatory acceptance floor—the same 75/30 ksi used for TP347, not an N-strengthened 80/35 grade. Actual mill test certificate values are often higher; design calculations should still use Table 4 unless the purchase order states higher guaranteed values that the mill has accepted in writing. Cite UNS S34751 wherever allowable-stress tables are consulted so fabricators do not pull a sister-grade strength line from memory.

Hardness: Table 4 does not list a hardness maximum for TP347LN as a separately mandated acceptance item. If hardness matters for fabrication or end-user acceptance, state the limit on the purchase order and verify it on the MTC; otherwise omit hardness as a mandatory acceptance item. Flattening or bend and tension run on a lot basis; supplementary tests apply only when listed on the PO.

Dimensions and Tolerances

Dimensional practice for austenitic stainless steel pipe ordered to SA-312 typically follows ASME B36.19 / B36.19M stainless-steel pipe schedules. Outside diameter and wall thickness are stated as NPS and schedule, or as OD and specified wall. Common schedules for TP347LN enquiry include Schedule 5S, 10S, 40S, and 80S. Other walls and non-standard OD/wall combinations are available by agreement when both the mill and the order accept them.

Size coverage in commercial practice is summarized below. Confirm large NPS and heavy walls against mill capability for the chosen manufacturing type before you lock the purchase order.

  • NPS / DN: commonly from NPS 1/8 upward; large NPS and heavy walls depend on manufacturing type (SML versus WLD/HCW) and mill capability—confirm on enquiry
  • Schedules: 5S, 10S, 40S, 80S and special walls by agreement
  • Length: single random (SRL), double random (DRL), or fixed cut lengths as stated on the purchase order
  • Ends: plain end (PE), beveled end (BE), or other end preparations by agreement

Wall-thickness variation limits from SA-312 Table 3 (t/D = specified wall / ordered OD) are the acceptance bands used on mill test certificates and receiving inspection for TP347LN:

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

Source: SA-312 Table 3; outside diameter variations per A999/A999M. OD, wall, and length tolerances follow SA-312 via ASTM A999/A999M and the dimensional standard on the order. SHH STEEL quotes the applicable clause rather than dumping entire A999 tables. Confirm max wall and NPS near the edge of B36.19 practice before acceptance.

Equivalent Grades

Equivalence for TP347LN must be stated carefully. Chemistry approximations across regional designations help material selection discussions; they are not automatic one-to-one substitutes for ASME pressure-code pipe without an approved material specification and design-code acceptance.

Designation Notes
ASME SA-312 / ASTM A312 Grade TP347LN Governing pipe product standard for this article
UNS S34751 Unified number listed in Table 1
TP347 (UNS S34700) Sister Nb-stabilized grade; higher carbon ceiling and footnote G Nb rule—not LN
TP347H (UNS S34709) H grade for elevated temperature; different C band and grain-size practice
TP348 / TP348H Related Nb+Ta stabilized family; order the exact TP name on the PO

Within SA-312, do not interchange TP347LN with TP347 or TP347H on a shared “347” market label—each has its own Table 1 and Table 4 rows. Related pages: ASME SA312 TP347 Stainless Steel Pipe, ASME SA312 TP347H Stainless Steel Pipe, ASME SA312 TP348 Stainless Steel Pipe, ASME SA312 TP321 Stainless Steel Pipe. Hub: ASME SA 312/SA 312M.

Pressure-code caution: EN/JIS or proprietary approximations do not authorize B31 or Section VIII substitution without engineered approval and an accepted material specification written on the design documents.

Heat Treatment and Delivery Condition

All pipe furnished to ASME SA-312 shall be heat treated. For TP347LN and other grades that do not carry an individual temperature row in Table 2, the default minimum solution-annealing temperature is 1900 °F [1040 °C], followed by water quenching or another rapid cool sufficient to prevent harmful carbide reprecipitation. That Table 2 default is SHH STEEL’s delivery baseline unless the ordered edition of SA-312 states otherwise for the heat.

TP347LN is not an H grade. H-grade grain-size control and reheating notes written for TP347H do not change this LN heat-treatment path. Supplementary requirement S6 (stabilization heat treatment for the 321/347/348 family) applies only when the purchase order specifies it—do not assume S6 on every TP347LN shipment. HCW cold reduction is done before final anneal; delivery remains the annealed condition—cold work is not a final hardness condition.

Commercial delivery condition for TP347LN typically includes the following items unless the purchase order or ordered edition of SA-312 states otherwise:

  • Solution annealed to SA-312 Table 2 requirements for TP347LN
  • Pickled and descaled, or bright annealed, as ordered (see Surface Finishes)
  • Straightened and cut to the ordered length practice
  • Hydrotested or NDE-tested per length as required by the standard and the purchase order

Corrosion Resistance

TP347LN is selected for welded aqueous or sensitizing service where ultra-low carbon, niobium stabilization, and controlled nitrogen are accepted by the end-user specification without requiring molybdenum. The low carbon band and Nb ≥15×C rule are aimed at resisting carbide precipitation in the weld heat-affected zone. SA-312 itself does not publish corrosion rates for TP347LN—fitness for a given fluid, temperature, and velocity must be validated against the project corrosion specification, not inferred from the grade name alone.

Versus TP347 / TP347H: Tighter carbon and mandatory nitrogen make TP347LN a different chemistry package from ASME SA312 TP347 Stainless Steel Pipe or elevated-temperature ASME SA312 TP347H Stainless Steel Pipe. They are not automatic drop-in replacements when the datasheet fixed UNS S34751.

Versus Mo-bearing grades: When chloride pitting, crevice attack, or reducing media dominate, prefer molybdenum-bearing austenitics such as ASME SA312 TP316LN Stainless Steel Pipe or ASME SA312 TP316L Stainless Steel Pipe. Nb stabilization is not a substitute for Mo in chloride service.

Surface condition: Proper pickling and passivation after fabrication help restore a clean passive surface and remove free iron from handling. Mill annealed-and-pickled pipe already carries a descaled surface; site welding and grinding should be cleaned and passivated when the end-user specification requires it. Intergranular-corrosion or weld-decay testing is a supplementary requirement and applies only when written on the purchase order.

Applications of SA312 TP347LN Pipe

TP347LN pipe is selected where austenitic stainless behavior, SA-312 product form, and a low-carbon Nb–N chemistry are acceptable for the fluid and temperature—especially where welded construction and sensitization resistance matter more than molybdenum content. Typical application areas include:

Application area Typical use of TP347LN pipe Selection note
Welded process lines Aqueous or mildly corrosive transfer lines needing Nb stabilization with very low carbon Prove Nb ≥15×C and N band on the MTC
Chemical / refining utility Lines where 347-family chemistry is specified without H-grade or Mo requirements Prefer Mo grades if chlorides dominate
Heat-exchanger / condenser piping Where LN carbon control reduces HAZ sensitization risk after fabrication welding State finish, NDE, and any IGC tests on the PO
General corrosive service Mild to moderate environments ordered to SA-312 austenitic pipe Not a drop-in for TP316L/TP316LN in chloride service
Code piping packages Projects that dual-mark SA-312/A312 and keep heat traceability through fabrication Name edition year, manufacturing type, and UNS on the enquiry

When the same plant also uses other Nb-stabilized or low-carbon austenitic grades, buyers sometimes pair TP347LN with ASME SA312 TP347 Stainless Steel Pipe or ASME SA312 TP321 Stainless Steel Pipe—but only when each line’s datasheet actually allows that grade. Match the grade family to corrosion and code needs first; commercial convenience is secondary to fitness for service.

Weldability

TP347LN is generally weldable by common austenitic fusion processes with suitable heat input, interpass control, and joint cleanliness. Typical processes used on this grade include:

  • GTAW (TIG) — preferred for root passes and thin-wall pipe where weld metal cleanliness and heat-input control matter
  • GMAW (MIG) — productive for fill and cap passes on thicker walls when procedures are qualified
  • SMAW — widely used for field girth welds with coated austenitic electrodes selected by agreement
  • Automatic orbital or mechanized GTAW — common for repetitive high-integrity girth joints

With carbon locked at 0.005–0.020% and Nb required at ≥15×C, HAZ sensitization risk is lower than for higher-carbon 347 heats. Low heat input and controlled interpass remain good practice; they are engineering choices—not automatic SA-312 requirements on every order.

Filler metal: SA-312 Table 6 maps TP347LN to the ER347 family shared with other 347 grades. Qualify the AWS (or EN) classification on the WPS/PQR for the actual TP347LN base metal and freeze that class before production welds. Note that mill longitudinal welds for WLD and HCW product are made without filler metal; Table 6 guidance applies to joining with filler, not to the mill autogenous weld.

Girth welds follow the piping/vessel code (e.g. ASME B31 / Section IX) and are separate from mill hydro/NDE. Specify girth NDE on fabrication documents when required. Keep joints clean of oil, paint, and carbon-steel contamination.

Surface Finishes

Surface condition for SA312 TP347LN pipe is stated on the purchase order. Typical mill finishes available from SHH STEEL supply include the following options:

  • Annealed and pickled (AP) — solution annealed, descaled in acid pickle or an equivalent process, producing a matte gray finish common for process and utility pipe
  • Bright annealed (BA) — annealed in a protective atmosphere to a brighter surface where the order allows and mill capability exists for the size
  • Mechanically polished — for example 180#, 320#, or 400# grit, or Ra-controlled polish on OD and/or ID for hygienic or architectural duty; polishing does not replace solution annealing
  • Bead-finished welded OD — weld bead rolled or ground flush as agreed for WLD/HCW product

Passivation after pickle or polish can be added when the end-user specification requires it. For hygienic or high-purity lines, state both the Ra (or grit) target and the documentation package—including any surface roughness reports—on the enquiry. SHH STEEL will not imply a polished hygienic finish on standard AP pipe unless the purchase order says so. End preparation (plain or beveled) should be ordered together with finish so that bevel faces and ID cleanliness meet the same acceptance language.

Inspection and Testing

Base inspection and testing for SA-312 TP347LN pipe combines chemistry, mechanical, and integrity checks. The following items form the usual acceptance package; supplementary requirements apply only when written on the purchase order.

  • Heat (melting) analysis — mandatory per heat against Table 1 for TP347LN (UNS S34751), including C 0.005–0.020%, N 0.06–0.10%, Nb 0.20–0.50% and Nb ≥15×C
  • Product analysis — when ordered (Suppl. S1 / purchase-order language), using A480 Table A1.1 tolerances via A999 §6.3
  • Tension test — Table 4 tensile, yield, and elongation on a lot basis (75/30 ksi minima)
  • Flattening test — or alternate bend where the standard permits for certain welded pipe
  • Hydrostatic test or nondestructive electric test — each length; manufacturer’s option unless the order fixes the method
  • Visual and dimensional check — against ordered NPS/schedule or OD/wall and the applicable tolerance clauses

Mill test certificates: EN 10204 3.1 is the standard documentation package from SHH STEEL supply. EN 10204 3.2 or third-party witness (SGS, Bureau Veritas, TÜV, or the buyer’s nominated agency) is arranged when specified and should be booked before final testing. Dual ASME SA-312 / ASTM A312 certification is available when chemistry, heat treatment, mechanical tests, and marking satisfy the edition(s) named on the order.

Optional / supplementary: PMI, RT/UT, intergranular corrosion or weld-decay tests, tighter straightness, special marking—only when listed on the PO. Keep heat numbers on cut pieces for MTC traceability.

Packaging and Shipping

Export and domestic shipments of SA312 TP347LN pipe are packed for handling and ocean or land transport. Typical packing practices from SHH STEEL supply include:

  • Seaworthy bundles — pipes strapped or cradled in bundles sized for container or break-bulk handling, with separators where needed to protect finish
  • End caps / protectors — plastic or metal caps on plain or beveled ends to reduce damage and contamination during transit
  • Marking — durable marking of grade (TP347LN), UNS S34751 when required, heat number, size (NPS or OD × wall / schedule), manufacturing type (SML / WLD / HCW), and mill identity as required by SA-312 and the purchase order
  • Export packing — waterproof wrapping as agreed for polished or sensitive finishes; container stuffing photos on request

Segregate TP347LN from TP347 and TP347H on the packing list and in the yard so stencil mix-ups do not travel with the shipment. Shipment docs typically include packing list, invoice, B/L or AWB, and MTC (3.1 or 3.2), plus origin/customs papers per Incoterms. State destination, packing preference, and extra marking at enquiry.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless plate and pipe. For ASME SA312 TP347LN / UNS S34751 we quote against the edition you name, report the LN carbon–nitrogen–niobium window on the MTC (including footnote I’s Nb ≥15×C rule), and keep heat identity unbroken from melt through finished length—so receiving inspection clears the heat against Table 1 and Table 4 rather than against a vague “347LN” catalog sheet.

  • Specification fidelity — chemistry and tensile to SA-312/A312 Table 1 and Table 4 for TP347LN (S34751), not unpublished tighter windows
  • Mill resources — SML, WLD, and HCW from qualified stainless pipe mills with heat traceability
  • Documentation — EN 10204 3.1 MTCs standard; 3.2 or third-party inspection on request
  • Dual marking — ASME SA-312 and ASTM A312 when the heat and tests meet both requirements you name
  • Related grades — sister Nb-stabilized and low-carbon austenitic SA-312 grades when projects buy matched packages
  • Export packing — seaworthy bundles, end protectors, and durable grade/heat/size/type marking

Quotations follow your purchase-order language for edition year, manufacturing type, size, finish, and any supplementary tests you name. Grade hub: ASME SA 312/SA 312M.

Supply Capability

SHH STEEL can supply ASME SA312 TP347LN / UNS S34751 stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade.

Item SHH STEEL capability for TP347LN
Standard ASME SA-312/SA-312M and/or ASTM A312/A312M Grade TP347LN (UNS S34751)
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD/wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length SRL, DRL, or cut-to-length
Finish Annealed and pickled; bright annealed or polished by agreement
Testing Tension, flattening/bend, hydro or NDE per length; supplementary tests on order
Documents EN 10204 3.1; third-party inspection / 3.2 on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

Stock moves with mill rolling cycles. Enquiries should state the SA-312 edition, SML/WLD/HCW, NPS or OD×wall, length practice, and any product-analysis or 3.2 requirements so mill slots align with your need date. Cut lengths, beveling, and packing-list marking are available on confirmed orders.

FAQ

Is ASME SA312 the same as ASTM A312?
For chemistry (Table 1), tensile (Table 4), manufacturing types, and most testing language, ASME SA-312/SA-312M matches ASTM A312/A312M of the referenced edition. Dual SA312/A312 marking is common when ordered. Name both editions on the purchase order and mill test certificate so inspectors can verify the heat against the exact books you cited—do not assume a bare market grade stamp covers dual certification.
What is the UNS number for TP347LN?
Table 1 lists TP347LN as UNS S34751. Use that UNS on the purchase order, stencil, and MTC so chemistry and tensile rows stay unambiguous. When the project mixes plate and pipe, carry the same UNS language across forms, but still order pipe to SA-312/A312—not to the plate specification alone.
TP347LN vs TP347 — which should I order?
TP347LN tightens carbon to 0.005–0.020%, adds N 0.06–0.10%, and sets Nb 0.20–0.50% with footnote I (≥15×C). TP347 allows C ≤0.08% with footnote G Nb. Order the exact UNS. Put the design-code grade and UNS on the datasheet and purchase order before you compare price—switching to TP347 after fabrication drawings are frozen usually means a material change notice, not a free mill substitution.
TP347LN vs TP347H — which should I order?
TP347H is the H grade for elevated temperature with C 0.04–0.10% and grain-size control; TP347LN is a low-carbon nitrogen-bearing Nb grade without Table 5 mandates. Put the design-code grade and UNS on the datasheet and purchase order before you compare price—switching to TP347H after fabrication drawings are frozen usually means a material change notice, not a free mill substitution.
Seamless vs welded TP347LN — which is better?
Neither is universally better. Choose the manufacturing type your design code and datasheet allow; both are legitimate SA-312 forms when tested to the standard. State SML, WLD, or HCW on the purchase order and confirm the same letters on the pipe marking and MTC—mixing offers that differ only in manufacturing type is a common bid-evaluation trap.
Can you dual-certify SA312 / A312 TP347LN?
Yes, when heat analysis, heat treatment, mechanical tests, and marking meet both editions named on the order. Write the ASME and ASTM edition years on the PO, and require the MTC to reference both books so receiving inspection can clear the heat without a second paperwork chase after shipment.
Hydrostatic test vs NDE — which do I get?
Each length is hydrotested or nondestructively electrically tested. Manufacturer may choose unless the purchase order fixes the method. If your piping class or client specification locks one method, state it on the PO and verify the chosen test appears on the MTC for every length—silent mill option is not the same as an approved project method.
What heat treatment / anneal temperature applies to TP347LN?
Table 2 default 1900 °F [1040 °C]. Not an H grade. Supplementary S6 applies only when specified. Delivery remains the solution-annealed condition required by SA-312 unless the edition and PO state otherwise. Cite the ordered edition’s Table 2 row on the enquiry so the mill does not apply a neighboring grade’s anneal practice by habit.
What Table 1 chemistry defines TP347LN?
Table 1: C 0.005–0.020%, Cr 17.0–19.0%, Ni 9.0–13.0%, Nb 0.20–0.50% (and ≥15×C per footnote I), N 0.06–0.10% (UNS S34751). Values are melting-analysis limits from the ordered edition—do not invent tighter catalog windows. When product analysis is needed, order it explicitly (Suppl. S1 / PO language) rather than assuming ladle values alone will satisfy receiving inspection.
What are the Table 4 tensile requirements for TP347LN?
Table 4 minima are 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield (elongation per the standard’s Table 4 row). Actual MTC values are often higher; design still uses Table 4 unless the PO states higher guarantees. Record the Table 4 row on the datasheet so fabricators do not substitute a sister-grade strength line from memory.
What filler metal should I use to weld TP347LN pipe?
Table 6 maps to the ER347 family for TP347LN. Mill WLD/HCW welds use no filler. Qualify and freeze the AWS class on the WPS. Freeze the AWS (or EN) class on the WPS/PQR before production welds, and remember mill WLD/HCW longitudinal welds are autogenous—Table 6 guidance applies to joining with filler, not to the mill seam.
What carbon range does TP347LN require?
Table 1 requires carbon in the 0.005–0.020% band for S34751—tighter than TP347. Confirm both the minimum and maximum on the heat analysis. Confirm the limit against the ordered edition of SA-312/A312 and put the same wording on the purchase order and MTC review checklist so receiving inspection does not invent a tighter window.

Conclusion

ASME SA312 TP347LN (UNS S34751) is the low-carbon, nitrogen-bearing, niobium-stabilized austenitic pipe grade in SA-312 for welded service when the LN carbon band (0.005–0.020%), nitrogen 0.06–0.10%, and Nb 0.20–0.50% with ≥15×C are required. Table 4 minima are 75/30 ksi; heat treatment follows the Table 2 default 1900 °F [1040 °C]; Table 6 filler guidance is the ER347 family; it is not an H grade, and S6 applies only when specified. Order the manufacturing type (SML/WLD/HCW), schedule or wall, finish, and any product analysis or supplementary tests explicitly. For stock checks, mill certificates, or dual SA-312/A312 supply questions, contact SHH STEEL at admin@steelspecs.com or browse the ASME SA 312/SA 312M category on steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X