GB/T 714 Q500qNHD weathering bridge steel stacked at SHH STEEL warehouse

GB/T 714 Q500qNHD Weathering Bridge Steel Supplier

GB/T 714 Q500qNHD (Q500qDNH) is weathering bridge steel plate with 500 MPa minimum yield, 120 J Charpy at −20°C (12–100 mm), Cu-Cr-Ni chemistry and a weathering index I ≥6.0 for unpainted bridges. SHH STEEL supplies it mill-direct with Z15–Z35, UT and full heat and product analysis.
Keywords
Q500qNHD, Q500qNHD weathering steel, GB/T 714 Q500qNHD, Q500qDNH, Q500qDNH steel plate, Q500qNH, Q500qNHD weathering bridge steel, Q500qDNHZ15, Q500qDNHZ25, Q500qDNHZ35, bridge steel plate, Q500qNHD supplier
Equivalent Grades:
No direct equivalent in Annex B / closest: ASTM A709 HPS 70W (485 MPa) — Material Specification: GB/T 714-2025 (supersedes GB/T 714-2015) — Delivery: TMCP / TMCP+T
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q500qNH Quality Grades
GB/T 714-2025 vs 2015
Q500qNHD vs ASTM A709 / EN 10025
Weathering Index and Unpainted Use
Welding and Fatigue
Z15 / Z25 / Z35
Equivalent Material Grades
Testing and Inspection
Dimensions
Tolerances
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 714 Q500qNHD Weathering Bridge Steel?

Q500qNHD is weathering bridge structural steel to GB/T 714. In the standard’s own notation it is written Q500qDNH: Q for yield, 500 for the minimum yield in MPa, q for qiao (bridge), the quality letter, and NH for nai hou, weathering. The letter D means Charpy V-notch testing at −20°C.

Q500qNH is the strongest weathering bridge grade on our list, with a richer Cr-Ni-Cu band for heavy unpainted members. Q500qNH moves to Cr 0.45–0.70%, Ni 0.30–0.45%, Cu 0.25–0.55% and Mo ≤0.25%, which supports both strength and the weathering index. Pcm is capped at 0.24% to 50 mm.

Q500qNHD (Q500qDNH) is the strongest weathering bridge plate on our list with a −20°C Charpy. Its richer Cr-Ni-Cu band (Cr 0.45–0.70%, Ni 0.30–0.45%, Cu 0.25–0.55%) supports both strength and the weathering index.

GB/T 714-2025, in force since 1 May 2026, fully replaces GB/T 714-2015; the changes for weathering grades are listed below.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q500qNHD cut to size with an EN 10204 3.1 or 3.2 certificate. Sister grades are listed under GB/T 714; other unpainted options are under weathering steel plates and EN 10025-5.

Material Specification

Specification element Requirement SHH STEEL compliance
Standard GB/T 714-2025 Q500qDNH Confirmed
Product Single-rolled plate ≤150 mm; hot-rolled strip and cut plate ≤25.4 mm Plate
Thickness with tensile values Up to 130 mm for Q500qNH Confirmed
Minimum yield ReL 500 MPa ≤50 mm; 480 MPa >50–100 mm Confirmed
Minimum tensile Rm 630 MPa ≤100 mm (no upper limit in the standard) Confirmed
Elongation A ≥ 18% Confirmed
Charpy V-notch −20°C, 120 J (12–100 mm), longitudinal Confirmed
Weathering index I ≥ 6.0 (Table 5, footnote c) Calculated on MTC
Delivery condition TMCP or TMCP + tempering As ordered
Weldability index Pcm (Table 8) Printed on MTC
Ultrasonic testing Plate >20 mm: GB/T 2970, Class II or better Every plate
Through-thickness Z15, Z25 or Z35 to GB/T 5313, when ordered As ordered
Dimensions GB/T 709 Confirmed
Certificate GB/T 247; EN 10204 3.1 or 3.2 As ordered

Grades often compared with Q500qNHD are ASTM A709 HPS 70W and EN 10025-4 S460ML; the comparison below shows where they differ.

Chemical Composition: Heat Analysis and Product Analysis

Read the Q500qNHD certificate with two tables in mind: heat limits from GB/T 714 and product limits from GB/T 222. A plate can pass one and be argued over in the other if the basis is not written into the contract.

Table 1 below is the heat (ladle) analysis for Q500qNHD from GB/T 714-2025 Tables 1, 5.

Element Q500qNHD heat analysis (%) Note
C, max 0.11
Si 0.15 – 0.50 Counts in I
Mn 1.10 – 1.50 Min 0.50% for coil only
P, max 0.025 Letter D
S, max 0.015 Letter D
Cu 0.25 – 0.55 Main weathering element
Cr 0.45 – 0.70 Weathering element
Ni 0.30 – 0.45 Weathering element
Mo, max 0.25
Nb 0.010 – 0.100 Microalloy (see note)
V 0.010 – 0.100 Microalloy (see note)
Ti 0.006 – 0.030 Microalloy (see note)
Als 0.015 – 0.050 Alt 0.020–0.055% if total Al is used
N, max 0.0080
B, max (residual) 0.0005 ≤0.0014% if C ≤0.06%
H, max (residual) 0.0002
Weathering index I ≥ 6.0 Calculated from heat analysis

Nb, V, Ti and Al may be added singly or together. Added singly, each must meet the range above; added together, at least one must reach its minimum and Nb + V + Ti ≤ 0.22%. Calcium treatment is required to control sulfide shape.

Table 2 is the product analysis: the limits a check analysis on finished plate is judged against. GB/T 714-2025 clause 7.1.3 calls up GB/T 222 for the permitted deviations.

Element Heat limit (%) Deviation, GB/T 222-2025 Table 1 Q500qNHD product analysis (%)
C ≤ 0.11 +0.02 ≤ 0.13
Si 0.15 – 0.50 ±0.05 0.10 – 0.55
Mn 1.10 – 1.50 ±0.06 1.04 – 1.56
P ≤ 0.025 +0.005 ≤ 0.030
S ≤ 0.015 +0.005 ≤ 0.020
V 0.010 – 0.100 +0.02 / −0.01 ≤ 0.120
Ti 0.006 – 0.030 +0.02 / −0.01 ≤ 0.050
Nb 0.010 – 0.100 ±0.005 (listed for 0.015–0.060%) Above 0.060%: agree in contract
Cu 0.25 – 0.55 ±0.05 0.20 – 0.60
Cr 0.45 – 0.70 ±0.05 0.40 – 0.75
Ni 0.30 – 0.45 ±0.05 0.25 – 0.50
Als 0.015 – 0.050 ±0.003 Lower limit −0.003 (Table 1 row is for Al ≥0.015%; confirm)
Mo ≤ 0.25 Not listed in Table 1 Agree in contract
N ≤ 0.0080 Listed only for 0.010–0.020% Agree in contract

How to read Table 2. Weathering bridge steel is normally classed as low-alloy steel, so Table 1 of GB/T 222 applies. Where the heat limit is a range, the deviation applies to both ends; for one heat, an element may deviate in one direction only.

Mechanical Properties

Tensile values follow Table 9 of GB/T 714-2025 for Q500qNH. Tensile specimens are transverse; round specimens are used above 40 mm. Where yield is not distinct, Rp0.2 replaces ReL.

Nominal thickness ReL min (MPa) Rm min (MPa) A min
≤ 50 mm 500 630 18%
> 50 – 100 mm 480 630 18%
> 100 – 130 mm 450 560 18%

Impact values follow Table 10, on longitudinal specimens, average of three:

Letter / test temperature KV2 ≤12 mm KV2 >12 – 100 mm KV2 >100 – 150 mm
D / −20°C 80 J 120 J 47 J

One single value may fall below the required average, but not below 70% of it. Plate over 8 mm and under 12 mm is tested with 7.5 mm specimens (75% of the value); 6–8 mm plate with 5 mm specimens (50%). Plate under 6 mm is not impact tested.

180° bend test, transverse: mandrel D = 2a up to 16 mm and 3a above 16 mm; may be omitted when the mill guarantees it. Yield ratio is not mandatory. If the contract asks for it, Annex C recommends ReL/Rm ≤ 0.88 up to 12 mm and ≤ 0.86 above 12 mm for TMCP plate.

Q500qNHD / Q500qNHE / Q500qNHF: Which Quality Grade?

Q500qNHD is tested at −20°C. It suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C. D is the most specified letter on Chinese bridge drawings. It is tested at −20°C and the melt is tighter than C: P ≤0.025%, S ≤0.015%.

Grade Test temp. KV2 ≤12 mm KV2 12–100 mm KV2 >100 mm P / S max (%)
Q500qNHD −20°C 80 J 120 J 47 J 0.025 / 0.015
Q500qNHE −40°C 80 J 120 J 31 J 0.020 / 0.010
Q500qNHF −60°C By agreement 54 J — 0.015 / 0.006

Over-specifying the letter costs money; under-specifying it costs safety. Choose from the lowest service or erection temperature, then step up one letter for thick, restrained or fracture-critical members.

Q500qNHD: What Changed from GB/T 714-2015 to GB/T 714-2025

For Q500qNHD buyers the 2025 edition changes more than the year on the certificate. The points below come from the foreword of GB/T 714-2025 and its tables.

  • The weathering requirement changed: Table 5 now requires a corrosion index I ≥ 6.0, and the 2015 Annex C guide for assessing weathering resistance was deleted.
  • A Pcm table for weathering steel (Table 8) was added.
  • Annex A now gives reference bridge-site environments for unpainted use (chloride, SO₂ and time-of-wetness limits).
  • Yield values above 100 mm were added for Q500qNH (450 MPa for >100–130 mm).
  • Tensile strength is now banded by thickness (e.g. lower minimum Rm above 100 mm) instead of one value.
  • Impact energy is set by thickness band (≤12 mm, 12–100 mm, >100 mm) in Table 10.
  • Yield ratio is no longer a clause value; it is agreed in the contract, with recommendations in informative Annex C.

If a drawing cites 2015 and the plate is made to 2025, get the designer’s written acceptance; tensile strength above 100 mm and the yield-ratio basis differ.

Q500qNHD vs ASTM A709 and EN 10025: Which Grade Matches?

Can Q500qNHD replace a US or European bridge grade, or the other way round? Strength can match; toughness rules differ in kind, not only in number.

Property Q500qNHD ASTM A709 HPS 70W EN 10025-4 S460ML
Min. yield (MPa) 500 (≤50 mm) 485 460 (≤16 mm)
Tensile (MPa) 630 min 585 – 760 540 – 720
Charpy 120 J at −20°C (12–100 mm) CVN by temperature zone; fracture-critical (F) levels 27 J at −50°C
Weathering chemistry Yes, I ≥ 6.0 Yes No

ASTM A709 sets Charpy requirements by temperature zone (1, 2, 3) and by member type: non-fracture-critical (T) or fracture-critical (F). GB/T 714 sets one value per letter, so compare the A709 zone with the GB/T 714 test temperature, not grade with grade.

EN 10025-5 weathering grades are general structural steels without a bridge-specific toughness level of 120 J; they suit many bridges but are not a one-to-one match.

The 120 J requirement for 12–100 mm plate is several times the 27–40 J typical of general weathering grades such as ASTM A588 or Corten A/B plate, which is why bridge owners specify Q500qNHD.

Q500qNHD Atmospheric Corrosion Index I and Unpainted Bridges

GB/T 714-2025 Table 5, footnote c, requires every Q500qNHD heat to reach an atmospheric corrosion index I of at least 6.0, calculated from the heat analysis:

I = 26.01(%Cu) + 3.88(%Ni) + 1.20(%Cr) + 1.49(%Si) + 17.28(%P) − 7.29(%Cu)(%Ni) − 9.10(%Ni)(%P) − 33.39(%Cu)²

This is the same predictive formula used with ASTM G101 for ASTM A709 Grade 50W and ASTM A709 HPS 70W, which makes Chinese and US ASTM A709 weathering steel plates easy to compare with Q500qNHD.

Worked example (our calculation) Cu Ni Cr Si P I
All weathering elements at their Table 5 minimum 0.25 0.30 0.45 0.15 0.010 5.94
Illustrative mid-range heat 0.32 0.36 0.55 0.30 0.012 6.74

Note the first row: a heat that only just meets every Table 5 minimum can still fall short of I = 6.0. That is why we ask the mill to print I on every Q500qNHD certificate, not just the chemistry.

Where can the steel be left unpainted? Annex A of GB/T 714-2025 gives reference bridge-site conditions:

  • Rural or urban atmosphere with annual chloride deposition ≤ 3 mg/(m²·d)
  • Annual SO₂ deposition ≤ 24 mg/(m²·d)
  • Time of wetness ≤ 5,256 h per year (temperature above 0°C and relative humidity above 80%)
  • Coastal sites only if they meet the same limits; for marine atmospheres Annex D points to T/CISA 073

The patina on Q500qNHD needs wet-dry cycles. Members that stay damp, such as those under leaking joints or close to vegetation, rust like ordinary steel. Plan inspection access in the first five years.

Welding Q500qNHD and Fatigue in Bridge Girders

GB/T 714-2025 clause 7.1.2 uses CEV for normalized, QT and TMCP steel with C >0.12%, and Pcm for weathering steel and TMCP steel with C ≤0.12%, both from the heat analysis:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Index ≤50 mm >50–100 mm >100–130 mm
Pcm, Q500qNH (Table 8) ≤ 0.24 ≤ 0.26 By agreement

For Q500qNHD, ask the fabricator which index the WPS was qualified on. Where the WPS uses CEV and the standard uses Pcm, we print both on the certificate. At −20°C, most procedures qualified on TMCP plate pass HAZ impact without special measures; keep multi-wire SAW heat input inside the qualified band.

Typical consumables for Q500qNHD: weathering-matched Ni-Cu consumables (AWS E8018-W2 type for 345–420 MPa), with higher-strength weathering wires for 460–500 MPa.

Fatigue. Welded details govern fatigue life in a bridge, and their fatigue strength is set by detail category, not by yield strength. Higher-strength plate can carry higher stress ranges only if detailing improves too.

Fatigue design follows JTG D64 (highway) and TB 10091 (railway) in China, EN 1993-1-9 in Europe and AASHTO LRFD in the US; fabrication commonly follows TB 10212, JTG/T 3650 or AWS D1.5.

Q500qDNHZ15, Z25 and Z35: Through-Thickness Plate for Bridges

Through-thickness properties matter wherever a full-penetration weld sits on the face of a plate, such as diaphragm-to-flange joints and cable anchor plates.

GB/T 714 adds the Z level to the end of the designation, for example Q500qDNHZ25. The test and acceptance follow GB/T 5313 and apply to plate 15 mm and thicker.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

D chemistry allows S up to 0.015%. Z15 needs S ≤0.010% and Z25 needs ≤0.007%, so Z plate is still made from a dedicated low-sulfur heat.

Put Z only where the joint needs it, usually node plates, anchor boxes and diaphragm-to-flange joints over about 25 mm. Keep the rest standard Q500qNHD. Z options apply across the GB/T 714 bridge steel range.

Equivalent Material Grades

Annex B of GB/T 714-2025 lists foreign grades against each strength level. It is informative: it tells you which families are close, not that the plates are interchangeable.

Standard Grade(s) Fit for Q500qNHD
ASTM A709 ASTM A709 HPS 70W Listed against Q460q in Annex B
EN 10025-4 EN 10025-4 S460ML Strength match, not weathering
EN 10025-6 EN 10025-6 S460QL QT, not weathering
GB/T 714 (painted twin) Q500qD Same strength, no weathering elements

For weathering grades also compare the corrosion index basis. Q500qNHD requires I ≥ 6.0 by the formula above; check that the substitute is assessed on the same basis.

Q500qNHD Testing, UT and Certificate

A batch of Q500qNHD is one grade, one heat, one thickness, one rolling schedule and one heat-treatment condition, up to 60 t. Table 12 of GB/T 714-2025 sets the tests:

Test Frequency Method
Heat analysis 1 per heat GB/T 20066; GB/T 4336 / GB/T 223
Weathering index I Calculated per heat Table 5 formula
Tensile 1 per batch GB/T 2975 / GB/T 228.1
Bend 180° 1 per batch (may be waived if guaranteed) GB/T 232
Charpy V at −20°C 3 specimens per batch GB/T 229
Through-thickness (Z) 3 specimens per batch, when ordered GB/T 5313
Ultrasonic Every plate >20 mm, Class II or better GB/T 2970
Surface and dimensions Every plate Visual and gauges

Impact retest: if a set fails, three more specimens are taken from the same batch. The average of all six must meet the requirement; two values may be below it, but only one below 70%. At −20°C the 120 J level is comfortable for well-made TMCP plate, but we still check each batch value, not just the average.

Dimensions

Q500qNHD plate sizes we regularly ship:

  • Thickness: 6 mm – 130 mm under GB/T 714 tensile tables; most orders 10 – 80 mm
  • Width: 1500 – 4000 mm, depending on mill and thickness
  • Length: 6000 – 18000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, 7.85 g/cm³

Deck plate, webs, flanges, diaphragms and stiffeners are cut to drawing. For U-ribs and rolled sections on the same bridge, see steel beam profiles and steel structural profiles.

Tolerances

Dimensional tolerances for Q500qNHD follow GB/T 709, as GB/T 714 directs. The default is Class B, which fixes the minus side at 0.30 mm.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Bridge fabricators often ask for Class C (zero minus) on deck and flange plate so section properties are never under the design value. Wider plates follow the heavier GB/T 709 rows; we state them on the offer.

Q500qNHD Price Factors and How to Order

Price questions on Q500qNHD usually come down to the extras in the table below.

Cost driver Effect on price
Strength level Q500q Higher levels need more alloy and tighter rolling control
Quality letter Small extra for −20°C testing and cleaner melt
Weathering alloys Cu, Cr, Ni additions and I-index control add a weathering extra
Delivery route TMCP / TMCP+T
Thickness Over 60 mm and under 10 mm carry size extras
Z15 / Z25 / Z35 Low-sulfur heat, Z test, UT; Z35 costs most
Width and length Over 3000 mm wide or 15 m long needs mill confirmation
Quantity per size Mill minimums per heat and size
Inspection and processing 3.2 witness, profile cutting, blasting, priming quoted per item

To get a firm quote in one round, send:

  • Grade, edition and Z level, e.g. Q500qDNHZ25 to GB/T 714-2025
  • Thickness × width × length and pieces or tonnes
  • Delivery route and UT class if beyond Class II
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line. Need another letter? See Q500qNHE, Q500qNHF.

Applications

Sector Typical Q500qNHD components
Unpainted highway bridges Plate girders and box girders in rural and urban atmospheres
Railway bridges Truss members, plate girders, bracing
Remote and mountain sites Bridges where repainting access is difficult or costly
Urban viaducts Exposed girders with architectural rust finish
Pedestrian bridges Unpainted box sections

The letter D suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C.

Q500qNHD is the wrong plate for marine splash zones, tunnels, sites with heavy de-icing salt spray, or members that stay wet. There, use painted Q500qD or look at marine-atmosphere grades under T/CISA 073.

Supply Capability and Global Delivery

SHH STEEL sources Q500qNHD from first-line bridge-plate mills, including drafters of GB/T 714-2025 such as Ansteel, Valin Xiangtan, Jiangyin Xingcheng, Wuyang, Shougang and Xinyu.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness (SGS, BV, TÜV or owner’s inspector)
  • Tests: tensile, −20°C Charpy, bend, Z test, UT, product analysis, weathering index
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blasting and priming (or blasting only, for unpainted weathering steel)
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill, per GB/T 247

We ship Q500qNHD to fabricators in Asia, Africa, the Middle East, Europe and the Americas, by break-bulk or container.

Lead time: about 45–60 days from mill rolling; Z35, F letter or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Southeast Asia and 28–35 days to North Europe.

Why Choose SHH STEEL

As a steel manufacturer and exporter and global steel mill sourcing partner, SHH STEEL buys Q500qNHD straight from GB/T 714 mills, China origin. No mixed heats, no relabelled plate.

Before shipment we check four lines on every Q500qNHD certificate: yield and tensile for the actual thickness band, Charpy at −20°C, the Pcm and weathering index, and UT results. If one fails, the plate does not ship as Q500qNHD.

Q500qNH is rarely in stock. Plan for mill rolling and include the weathering index and Pcm on the certificate requirements.

We also tell buyers when another grade fits better. Neighbouring levels are Q460qNHD. The painted counterpart is Q500qD. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q500qNHD steel?
Q500qNHD (Q500qDNH) is weathering bridge steel plate to GB/T 714-2025. It has 500 MPa minimum yield up to 50 mm, 630 MPa minimum tensile, Charpy impact of 120 J at −20°C for 12–100 mm plate, and Cu-Cr-Ni chemistry with a corrosion index I of at least 6.0 for unpainted bridges.
What is the difference between Q500qNHD and Q500qNHE?
Strength and chemistry box are the same. Q500qNHD is Charpy tested at −20°C, Q500qNHE at −40°C, both needing 120 J for 12–100 mm plate. P/S caps are 0.025/0.015% for D and 0.020/0.010% for E. Choose by the lowest service or erection temperature.
Is Q500qNHD the same as Q500D?
No. Q500D is general structural steel (GB/T 1591), while Q500qNHD is bridge steel to GB/T 714 with lower P and S, controlled weldability index, mandatory UT above 20 mm and 120 J impact for 12–100 mm plate. Bridge plate can replace general plate, not the reverse.
What is the ASTM or EN equivalent of Q500qNHD?
Close grades for Q500qNHD: No direct equivalent in Annex B / closest: ASTM A709 HPS 70W (485 MPa). These are close families, not drop-in substitutes; compare yield at thickness, impact temperature and energy, and the weldability index before substituting.
What is the batch size for GB/T 714 bridge plate testing?
Up to 60 t of one grade, heat, thickness, rolling schedule and heat-treatment condition. Each batch gets one tensile test, one bend test and one set of three Charpy specimens; heat analysis is reported per heat.
Does Q500qNHD weathering steel need painting?
Not if the bridge site and details suit it. GB/T 714-2025 Annex A gives reference conditions for unpainted use: annual chloride deposition ≤3 mg/(m²·d), SO₂ ≤24 mg/(m²·d) and time of wetness ≤5,256 h per year. Marine splash zones and salt-sprayed members still need protection.

Conclusion

Q500qNHD to GB/T 714 is weathering bridge steel with 500 MPa minimum yield, Cu-Cr-Ni chemistry, a weathering index of at least 6.0 and 120 J Charpy at −20°C for 12–100 mm plate.

The next strength level is Q460qNHD, with Q500qNHE and Q500qNHF as sister letters. Choose the letter from the lowest service or erection temperature, here −20°C, and step up a letter for thick, restrained or fracture-critical members.

SHH STEEL ships Q500qNHD with heat analysis, weldability index and mechanical results on every certificate. Third-party inspection, product analysis and Z testing are added on request.

We ship from Shanghai to bridge builders worldwide. Browse the full GB/T 714 range or other weathering steel plates.

Share your size list, Z level and edition, and we reply with mill, route, lead time, test plan and price in one message. Contact SHH STEEL for a mill-direct Q500qNHD weathering bridge steel quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X