Q390GNH Steel Plate | GB/T 4171 GNH Weathering Steel
What is Q390GNH steel plate?
Q390GNH belongs to the high weathering (GNH) track associated with GB/T 4171 purchasing. GNH grades are typically selected for vehicles, containers, buildings, towers and similar structures where atmospheric corrosion resistance is emphasized relative to the low-P weldable NH series.
Designation note: Q390GNH is written here because buyers search and RFQ it under the GB/T 4171 hub. Source basis: GB/T 4171-2000 legacy / market. Confirm whether the contract edition is GB/T 4171-2008 (prefer Table 3 grades such as Q295GNH / Q355GNH) or an agreed mill chemistry matching this market name. The MTC governs.
Quality levels A-E may be ordered when impact testing is required; for high-weathering steel, impact may be waived by agreement under GB/T 4171-2008. Keep quality letters on this page as notes, not separate products.
SHH STEEL is a China mill-direct source for GB/T 4171 weathering plates. Category hubs: Weathering Steel Plates · GB/T 4171.
For better weldability at similar strength talk tracks, see NH grades: Q235NH · Q295NH · Q355NH · Q415NH · Q460NH · Q500NH · Q550NH. Other GNH pages: Q235GNH · Q295GNH · Q345GNH · Q390GNH · Q355GNH.
Material Specification for Q390GNH
| Parameter | Specification |
|---|---|
| Standard | GB/T 4171 (edition as ordered; primary reference GB/T 4171-2008) |
| Grade | Q390GNH (quality levels A-E as ordered, e.g. Q390GNHD) |
| Family | High weathering (GNH, elevated P) |
| Product form | Plate / strip (hot-rolled) |
| GB thickness limit (plate/strip) | ≤ 20 mm (larger by agreement) |
| SHH supply thickness | Typically ≤20 mm unless agreed; confirm mill |
| Width | 1500-4000 mm (confirm for thin strip) |
| Length | 6000-16000 mm; cut-to-size on request |
| Delivery condition | As-rolled / controlled-rolled / normalized as agreed |
| Surface | As-rolled or shot blasted |
| Edge | Mill edge or cut edge |
| Certification | EN 10204 3.1 / 3.2 |
| Dimensional standard | GB/T 709 (hot-rolled plate/strip) |
| Density | 7.85 g/cm³ |
Chemical Composition of Q390GNH (ladle analysis)
Ladle (heat) analysis limits below follow GB/T 4171-2000 legacy / market. Product analysis tolerances follow GB/T 222. Always verify the mill test certificate before fabrication or substitution.
| Grade | C | Si | Mn | P | S | Cu | Cr | Ni | Ti | RE |
|---|---|---|---|---|---|---|---|---|---|---|
| Q390GNH | ≤0.12 | 0.15-0.65 | ≤1.40 | 0.07-0.12 | ≤0.035 | 0.25-0.55 | – (not mandatory in 2000 Q390GNH) | – | ≤0.10 | ≤0.12 (addition) |
- Chemistry from GB/T 4171-2000 Table for Q390GNH. Confirm on MTC; not listed in GB/T 4171-2008 Table 3.
Optional micro-alloying per GB/T 4171: Nb 0.015-0.060%, V 0.02-0.12%, Ti 0.02-0.10%, Alt ≥0.020% (at least one reaches its lower limit when used in combination). Mo ≤0.30%, Zr ≤0.15% may be added. For Q415NH-Q550NH, Nb+V+Ti total ≤0.22%.
NH vs GNH: NH (weldable weathering) keeps phosphorus low (typically ≤0.025-0.030%) for better weldability. GNH (high weathering) intentionally elevates phosphorus to accelerate and densify the protective patina. Do not treat NH and GNH as interchangeable without a chemistry and fabrication review.
Mechanical Properties of Q390GNH (including quality levels A-E)
Tensile requirements for Q390GNH under GB/T 4171-2000 legacy / market. When yield is not pronounced, Rp0.2 may be used. Quality levels A-E stay on the same product page: they change Charpy temperature/energy, not the base grade chemistry table.
| Thickness (mm) | Yield ReL (MPa) | Tensile Rm (MPa) | Elongation A (%) |
|---|---|---|---|
| Hot-rolled (2000 table) | ≥390 | ≥490 (GB/T 4171-2000 hot-rolled) | ≥22 |
Bend test: 180°: d=a (≤6 mm); d=2a (>6 mm) per GB/T 4171-2000.
GB/T 4171-2008 Table 5 (longitudinal Charpy V-notch, 10x10x55 mm). Quality letter is part of the ordered designation (e.g. Q355NHD). High-weathering GNH grades may omit impact by agreement.
| Quality level | Test temperature | Min average KV2 |
|---|---|---|
| A | 20 °C | ≥ 47 J |
| B | 0 °C | ≥ 34 J |
| C | -20 °C | ≥ 34 J |
| D | -40 °C | ≥ 27 J |
| E | -40 °C | ≥ 27 J |
Source note: Mechanical values shown are from the cited edition or market practice. If the purchase order cites GB/T 4171-2008 only, prefer a 2008 Table 3/4 grade (for example Q355GNH instead of legacy Q345GNH) or obtain written mill agreement and MTC values.
Density is approximately 7.85 g/cm³.
Delivery Conditions for Q390GNH plate
As-rolled / controlled-rolled / normalized as agreed. Not quenched and tempered.
Hot-rolled weathering plates are normally supplied as-rolled. Controlled rolling (TMCP) or normalizing is used when toughness, thickness or fabrication needs require it. Normalization, when applied, is typically in the 900-950 °C range followed by air cooling, subject to mill practice.
Surface may be as-rolled or shot blasted. Stress relieving after fabrication is available when the purchaser specifies it. SHH STEEL supplies the delivery condition named on the order.
Weldability of Q390GNH weathering steel
Q390GNH is a high-phosphorus GNH grade. Elevated P improves patina behaviour but increases the need for disciplined hydrogen control, preheat practice and procedure qualification, especially on thicker sections and highly restrained joints.
Qualify SMAW / GMAW / SAW procedures on production-representative chemistry. Prefer low-hydrogen consumables and consumables selected for weathering service when bare exposure of welds is intended. Do not assume an NH WPS automatically covers GNH heats. If weldability is the project’s stronger constraint, evaluate sibling NH grades such as Q355NH or Q235NH.
Dimensional Tolerances for Q390GNH
Hot-rolled plate and strip dimensional tolerances follow GB/T 709 unless the order cites another dimensional standard. Width and length tolerances are normally agreed as plus-only or per GB/T 709 tables. Flatness follows the ordered class; tighter flatness and cut-to-size plates with edge preparation are available on request.
Respect the GB/T 4171 thickness window for this grade (plate/strip ≤ 20 mm unless otherwise agreed). SHH STEEL can supply cut-to-size plates within the agreed thickness range.
Applications and service limits for Q390GNH
Typical applications for Q390GNH:
- Vehicles, containers and transport equipment
- Building exteriors, facade panels and landscape structures
- Towers and lightly to moderately welded outdoor frames
- Components where high atmospheric corrosion resistance and patina appearance matter
- Replacement RFQs historically calling SPA-H / Corten A / A242 Type 1 style high-P chemistry (confirm match)
The self-protecting patina can lower long-term maintenance versus painted carbon steel in many rural and industrial atmospheres. It is not a universal coating substitute: sheltered pockets that stay wet, aggressive chloride splash, and continuous immersion often need coating or another material. Bridge projects that cite GB/T 714 weathering bridge steel should not be auto-filled with GB/T 4171 grades.
Related pages: Weathering Steel Plates · A242 Type 1 · Corten A · Corten B · S355J2W · S355J2WP · A588 Gr.A · A709 50W.
Atmospheric exposure guidance for Q390GNH
Bare Q390GNH is intended for atmospheres where a stable patina can form and dry periodically. Use the table as a selection aid; final coating or grade choice still follows the project specification.
| Environment | Typical fit for bare weathering plate | Note |
|---|---|---|
| Rural / mild industrial | Usually suitable | Needs wet/dry cycles for patina |
| Urban / general industrial | Often suitable | Check local pollution and design details |
| Coastal / marine splash with moderate chloride | Use with caution | May need coating, higher-Ni practice, or another grade |
| Sheltered pockets that stay wet | Not preferred bare | Design out traps or coat locally |
| Continuous immersion / aggressive chloride | Not recommended bare | Select coated carbon steel or another material |
Equivalent and related grades for Q390GNH
These grades are commonly compared with Q390GNH. They are approximate, not automatic substitutes. Match chemistry, mechanical properties, toughness, thickness limits and the project specification before replacing one grade with another.
Legacy higher-strength high-P grade. Compare property-by-property with Q355GNH / Q415NH and foreign WP grades; do not auto-substitute.
| Standard / family | Grade | Relation | Product page |
|---|---|---|---|
| GB/T 4171 | Q390GNH | This page | – |
| EN 10025-5 | S355J0WP / S355J2WP (strength class dependent) | WP talk track | S355J2WP |
| JIS / ASTM / commercial | SPA-H / A242 Type 1 / Corten A | High-P approximate maps | A242 Type 1 · Corten A |
| GB/T 4171 | Q355GNH | Primary 2008 high-P plate grade | Q355GNH |
| Category | GB/T 4171 hub | All NH / GNH product pages | GB/T 4171 · Weathering Steel Plates |
Q390GNH vs Q355GNH vs Q415NH (selection aid)
These grades are often discussed together in purchasing. They are related weathering steels, not automatic substitutes.
| Item | Q390GNH | Q355GNH | Matching NH (weldable) |
|---|---|---|---|
| Family | High-P GNH | Primary 2008 high-P plate grade | Low-P NH |
| Source basis | GB/T 4171-2000 legacy / market | GB/T 4171-2008 | GB/T 4171-2008 NH series |
| Pages | This page | Q355GNH | Q355NH · Q295NH |
Why choose SHH STEEL for Q390GNH
- China mill-direct supply of Q390GNH weathering plate under the GB/T 4171 family
- EN 10204 3.1 mill test certificates; 3.2 and third-party inspection (SGS, TUV, BV, ABS) on request
- Supply thickness aligned to GB limits: Typically ≤20 mm unless agreed; confirm mill
- Cutting, beveling and shot blasting available to shorten fabrication lead time
- Full NH and GNH coverage under one supply chain: GB/T 4171 hub · Weathering Steel Plates
- International near-equivalents available when the project cites ASTM / EN / JIS instead: A242 Type 1, S355J2W, S355J2WP, Corten A, Corten B, A588
Supply, cutting and inspection for Q390GNH
| Item | SHH STEEL supply note |
|---|---|
| Thickness | Typically ≤20 mm unless agreed; confirm mill (GB plate/strip limit ≤ 20 mm unless agreed) |
| Size | Width 1500-4000 mm; length 6000-16000 mm; cut-to-size on request |
| Delivery condition | As-rolled / controlled-rolled / normalized as agreed. Not quenched and tempered. |
| Processing | Cutting, beveling, shot blasting available |
| Mill certificate | EN 10204 3.1 standard; 3.2 on request |
| Third-party inspection | SGS, TUV, BV or ABS can be arranged |
| Quotation needs | Grade + quality letter (e.g. Q390GNHD), thickness × width × length, quantity, delivery condition, inspection level |
FAQ
-
What does the quality letter mean on Q390GNHA / B / C / D / E?
- Quality levels set Charpy V-notch test temperature and minimum energy (GB/T 4171 Table 5). They are ordered as part of the grade name and documented on this page; they are not separate product URLs.
-
What is the difference between Q390GNH and Q390NH?
- Q390GNH is high-weathering GNH (elevated P). NH grades such as Q355NH keep phosphorus low for welding. See Q355NH.
-
What thickness can SHH supply for Q390GNH?
- Typically ≤20 mm unless agreed; confirm mill. The GB/T 4171 plate/strip limit for this designation is ≤ 20 mm unless otherwise agreed with the mill.
-
What is Q390GNH equivalent to?
- Legacy higher-strength high-P grade. Compare property-by-property with Q355GNH / Q415NH and foreign WP grades; do not auto-substitute. Substitution still requires project approval and MTC review.
-
Is Q390GNH quenched and tempered?
- No. Standard delivery is as-rolled, controlled-rolled or normalized, not quenched and tempered.
Request a quotation
Send grade and quality letter (for example Q390GNHD), thickness × width × length (or cut size), quantity, delivery condition (AR / normalized / controlled rolled), and any inspection requirement. SHH STEEL will return mill availability, certification scope and a quotation.
Contact: admin@steelspecs.com · +86-18939509537 · +86-021-62716097
More options: GB/T 4171 · Weathering Steel Plates · A242 Type 1 · S355J2W