Q500NH Steel Plate | GB/T 4171 Weathering Steel - SHH STEEL

Q500NH Steel Plate | GB/T 4171 NH Weathering Steel

Q500NH is a weldable atmospheric-corrosion-resisting structural steel under GB/T 4171. Compared with high-weathering GNH grades, NH keeps phosphorus low so shop welding and fabrication stay practical, while copper, chromium and nickel still support a protective patina in proper wet/dry outdoor exposure. SHH STEEL supplies Q500NH plate with EN 10204 3.1 (or 3.2) mill test certificates.
Equivalent Grades:
High-strength weldable weathering under GB/T 4171; international one-to-one maps are scarce. Compare property-by-property. Sibling pages under https://www.steelspecs.com/products-item/gb-t-4171/. Confirm against project specs.
Heat Treatment
As-rolled / controlled-rolled / normalized; quenched and tempered permitted for Q500NH per GB/T 4171-2008.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Atmospheric exposure guidance
Equivalent Material Grade
Q500NH vs related grades
Why choose Us
Our Service
FAQ
Conclusion

What is Q500NH steel plate?

Q500NH belongs to the weldable weathering (NH) series of GB/T 4171. The series is intended for vehicles, bridges, containers, buildings and other welded, bolted or riveted outdoor structures where atmospheric corrosion resistance is required and weldability matters more than the high-phosphorus GNH package.

Order the quality letter with the grade (A, B, C, D or E), for example Q500NHC or Q500NHD. Quality levels change Charpy V-notch test temperature and minimum energy; they stay on this product page and are not separate SKUs.

SHH STEEL is a China mill-direct source for GB/T 4171 weathering plates. Category hubs: Weathering Steel Plates · GB/T 4171.

If the project needs the high-phosphorus patina package instead, see the GNH pages: Q235GNH · Q295GNH · Q345GNH · Q390GNH · Q355GNH. Sibling NH grades: Q235NH · Q295NH · Q355NH · Q415NH · Q460NH · Q500NH · Q550NH.

Material Specification for Q500NH

Parameter Specification
Standard GB/T 4171 (edition as ordered; primary reference GB/T 4171-2008)
Grade Q500NH (quality levels A-E as ordered, e.g. Q500NHD)
Family Weldable weathering (NH)
Product form Plate / strip (hot-rolled)
GB thickness limit (plate/strip) ≤ 60 mm (larger by agreement)
SHH supply thickness 6-60 mm
Width 1500-4000 mm (confirm for thin strip)
Length 6000-16000 mm; cut-to-size on request
Delivery condition As-rolled / controlled-rolled / normalized; quenched and tempered permitted for Q500NH per GB/T 4171-2008
Surface As-rolled or shot blasted
Edge Mill edge or cut edge
Certification EN 10204 3.1 / 3.2
Dimensional standard GB/T 709 (hot-rolled plate/strip)
Density 7.85 g/cm³

Chemical Composition of Q500NH (ladle analysis)

Ladle (heat) analysis limits below follow GB/T 4171-2008. Product analysis tolerances follow GB/T 222. Always verify the mill test certificate before fabrication or substitution.

Grade C Si Mn P S Cu Cr Ni
Q500NH ≤0.12 ≤0.65 ≤2.0 ≤0.025 ≤0.030* 0.20-0.55 0.30-1.25 0.12-0.65**
  • *By agreement S may be ≤0.008%.
  • **By agreement Ni lower limit may be waived.
  • Nb+V+Ti total ≤0.22%.

Optional micro-alloying per GB/T 4171: Nb 0.015-0.060%, V 0.02-0.12%, Ti 0.02-0.10%, Alt ≥0.020% (at least one reaches its lower limit when used in combination). Mo ≤0.30%, Zr ≤0.15% may be added. For Q415NH-Q550NH, Nb+V+Ti total ≤0.22%.

NH vs GNH: NH (weldable weathering) keeps phosphorus low (typically ≤0.025-0.030%) for better weldability. GNH (high weathering) intentionally elevates phosphorus to accelerate and densify the protective patina. Do not treat NH and GNH as interchangeable without a chemistry and fabrication review.

Mechanical Properties of Q500NH (including quality levels A-E)

Tensile requirements for Q500NH under GB/T 4171-2008. When yield is not pronounced, Rp0.2 may be used. Quality levels A-E stay on the same product page: they change Charpy temperature/energy, not the base grade chemistry table.

Thickness (mm) Yield ReL (MPa) Tensile Rm (MPa) Elongation A (%)
≤16 ≥500 600-760 ≥18
>16-40 ≥490 600-760 ≥16
>40-60 ≥480 600-760 ≥15

Bend test: 180°: mandrel a (≤6 mm); 2a (>6-16); 3a (>16).

GB/T 4171-2008 Table 5 (longitudinal Charpy V-notch, 10x10x55 mm). Quality letter is part of the ordered designation (e.g. Q355NHD). High-weathering GNH grades may omit impact by agreement.

Quality level Test temperature Min average KV2
A 20 °C ≥ 47 J
B 0 °C ≥ 34 J
C -20 °C ≥ 34 J
D -40 °C ≥ 27 J
E -40 °C ≥ 27 J

Density is approximately 7.85 g/cm³.

Delivery Conditions for Q500NH plate

As-rolled / controlled-rolled / normalized; quenched and tempered permitted for Q500NH per GB/T 4171-2008.

Hot-rolled weathering plates are normally supplied as-rolled. Controlled rolling (TMCP) or normalizing is used when toughness, thickness or fabrication needs require it. Normalization, when applied, is typically in the 900-950 °C range followed by air cooling, subject to mill practice.

For Q500NH, GB/T 4171-2008 also allows quenched and tempered delivery. State Q+T explicitly on the purchase order when required; otherwise as-rolled / controlled-rolled / normalized is the usual path.

Surface may be as-rolled or shot blasted. Stress relieving after fabrication is available when the purchaser specifies it. SHH STEEL supplies the delivery condition named on the order.

Weldability of Q500NH weathering steel

Q500NH is in the low-phosphorus weldable weathering family. Common processes include SMAW, GMAW and SAW. Use a qualified WPS. Low-hydrogen consumables (for example E7018-class or weathering-matched wires/electrodes agreed with the welding engineer) are preferred for many structural joints. Preheat and interpass temperature follow thickness, carbon equivalent, joint restraint and the approved procedure.

Matching or undermatching consumables must be chosen so the weld metal’s atmospheric corrosion behaviour and strength meet the design intent. Post-weld heat treatment is not normally required for atmospheric-exposure structures, but may be specified for critical joints. Compared with GNH high-P grades, Q500NH is generally the more fabrication-friendly choice when extensive welding is planned.

Dimensional Tolerances for Q500NH

Hot-rolled plate and strip dimensional tolerances follow GB/T 709 unless the order cites another dimensional standard. Width and length tolerances are normally agreed as plus-only or per GB/T 709 tables. Flatness follows the ordered class; tighter flatness and cut-to-size plates with edge preparation are available on request.

Respect the GB/T 4171 thickness window for this grade (plate/strip ≤ 60 mm unless otherwise agreed). SHH STEEL can supply cut-to-size plates within the agreed thickness range.

Applications and service limits for Q500NH

Typical applications for Q500NH:

  • Highway and railway bridges (when GB/T 4171 NH is specified; bridge-dedicated GB/T 714 qNH grades are a separate track)
  • Welded building frames and outdoor industrial structures
  • Transmission and communication towers
  • Containers, vehicle frames and rolling-stock components
  • Architectural exteriors where weldable weathering chemistry is preferred

The self-protecting patina can lower long-term maintenance versus painted carbon steel in many rural and industrial atmospheres. It is not a universal coating substitute: sheltered pockets that stay wet, aggressive chloride splash, and continuous immersion often need coating or another material. Bridge projects that cite GB/T 714 weathering bridge steel should not be auto-filled with GB/T 4171 grades.

Related pages: Weathering Steel Plates · A242 Type 1 · Corten A · Corten B · S355J2W · S355J2WP · A588 Gr.A · A709 50W.

Atmospheric exposure guidance for Q500NH

Bare Q500NH is intended for atmospheres where a stable patina can form and dry periodically. Use the table as a selection aid; final coating or grade choice still follows the project specification.

Environment Typical fit for bare weathering plate Note
Rural / mild industrial Usually suitable Needs wet/dry cycles for patina
Urban / general industrial Often suitable Check local pollution and design details
Coastal / marine splash with moderate chloride Use with caution May need coating, higher-Ni practice, or another grade
Sheltered pockets that stay wet Not preferred bare Design out traps or coat locally
Continuous immersion / aggressive chloride Not recommended bare Select coated carbon steel or another material

Equivalent and related grades for Q500NH

These grades are commonly compared with Q500NH. They are approximate, not automatic substitutes. Match chemistry, mechanical properties, toughness, thickness limits and the project specification before replacing one grade with another.

High-strength weldable weathering under GB/T 4171; international one-to-one maps are scarce. Compare property-by-property.

Standard / family Grade Relation Product page
GB/T 4171 Q500NH This page –
EN 10025-5 S355J2W family (strength class dependent) W talk track S355J2W
ASTM A588 / A709 50W Related weathering role A588 · A709 50W
Commercial Corten B Often closer for NH/W discussions Corten B
Category GB/T 4171 hub All NH / GNH product pages GB/T 4171 · Weathering Steel Plates

Q500NH vs Q460NH vs Q550NH (selection aid)

These grades are often discussed together in purchasing. They are related weathering steels, not automatic substitutes.

Item Q500NH Q460NH Q550NH
Role GB/T 4171 NH Related GB/T 4171 grade Related GB/T 4171 grade
Min yield class 500 See page See page
Pages This page Q460NH Q550NH

Why choose SHH STEEL for Q500NH

  • China mill-direct supply of Q500NH weathering plate under the GB/T 4171 family
  • EN 10204 3.1 mill test certificates; 3.2 and third-party inspection (SGS, TUV, BV, ABS) on request
  • Supply thickness aligned to GB limits: 6-60 mm
  • Cutting, beveling and shot blasting available to shorten fabrication lead time
  • Full NH and GNH coverage under one supply chain: GB/T 4171 hub · Weathering Steel Plates
  • International near-equivalents available when the project cites ASTM / EN / JIS instead: A242 Type 1, S355J2W, S355J2WP, Corten A, Corten B, A588

Supply, cutting and inspection for Q500NH

Item SHH STEEL supply note
Thickness 6-60 mm (GB plate/strip limit ≤ 60 mm unless agreed)
Size Width 1500-4000 mm; length 6000-16000 mm; cut-to-size on request
Delivery condition As-rolled / controlled-rolled / normalized; quenched and tempered permitted for Q500NH per GB/T 4171-2008.
Processing Cutting, beveling, shot blasting available
Mill certificate EN 10204 3.1 standard; 3.2 on request
Third-party inspection SGS, TUV, BV or ABS can be arranged
Quotation needs Grade + quality letter (e.g. Q500NHD), thickness × width × length, quantity, delivery condition, inspection level

FAQ

What does the quality letter mean on Q500NHA / B / C / D / E?
Quality levels set Charpy V-notch test temperature and minimum energy (GB/T 4171 Table 5). They are ordered as part of the grade name and documented on this page; they are not separate product URLs.
What is the difference between Q500NH and Q500GNH?
Q500NH is weldable NH (low P). Q500GNH is high-weathering GNH (elevated P). See Q355GNH for the high-P track.
What thickness can SHH supply for Q500NH?
6-60 mm. The GB/T 4171 plate/strip limit for this designation is ≤ 60 mm unless otherwise agreed with the mill.
What is Q500NH equivalent to?
High-strength weldable weathering under GB/T 4171; international one-to-one maps are scarce. Compare property-by-property. Substitution still requires project ap
Is Q500NH quenched and tempered?
Q+T is permitted for this grade under GB/T 4171-2008 when ordered; otherwise AR / controlled-rolled / normalized is standard.

Request a quotation

Send grade and quality letter (for example Q500NHD), thickness × width × length (or cut size), quantity, delivery condition (AR / normalized / controlled rolled / Q+T), and any inspection requirement. SHH STEEL will return mill availability, certification scope and a quotation.

Contact: admin@steelspecs.com · +86-18939509537 · +86-021-62716097

More options: GB/T 4171 · Weathering Steel Plates · A242 Type 1 · S355J2W

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X