JIS G3463 SUS436LTB Stainless Steel Tube
What is JIS G3463 SUS436LTB Stainless Steel Tube
JIS G3463 covers both seamless and welded stainless tube for process, utility, condenser and heat-exchange duties. Inside that standard, SUS436LTB is filed as ferritic. If fresh-water 430LX still pits at crevices, JIS G3463 SUS436LTB is the Mo ferritic step before jumping to nickel austenitics. Buyers working Japanese boiler and HX packages should treat SUS436LTB as a governed product symbol under G3463, with Table 3 chemistry and Table 4 tensile floors enforced on the same heat. Corrosion framing beside SUS436LTB: Mo + stabilisation lifts pitting resistance in many waters vs 430LX.
From pierce/draw or weld-and-anneal through marking and bundle protection, SHH STEEL can produce JIS G3463 SUS436LTB for the sizes and tests on your RFQ. Application sketch: mild chloride coolers, automotive-adjacent exchangers, and ferritic HX needing a Mo bump. Size and test clarity on the RFQ lets SHH STEEL lock the correct Table 1 symbols for SUS436LTB before production starts. Size practice for SUS436LTB remains HX OD in standard practice; confirm Mo on MTC.
On the floor people shorten marks; in QA they must not. SUS436LTB under JIS G3463 carries specific Table 3 windows and Table 4 floors that a loose “436L Mo ferritic” note will not enforce. Caution: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex. Keep isometric notes, tubesheet specs, and the mill acknowledgement aligned on SUS436LTB so informal alias language cannot reopen the carbon or molybdenum window after melt. Corrosion framing beside SUS436LTB: Mo + stabilisation lifts pitting resistance in many waters vs 430LX.
Superheater, condenser and corrosive HX duties all sit in G3463’s scope statement; still match the alloy to the medium. For SUS436LTB, that means: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. Nearby marks: SUS444TB, SUS430J1LTB, SUS430LXTB, SUS316LTB. Document the medium, design temperature, and weld map beside the SUS436LTB line item so sister-grade swaps are engineering decisions rather than purchasing shortcuts. Size practice for SUS436LTB remains HX OD in standard practice; confirm Mo on MTC.
Inside this JIS G3463 series, compare SUS444TB, SUS430J1LTB, SUS430LXTB, SUS316LTB. Hub: JIS G3463. ASTM/ASME related product pages (not interchangeable by default): ASTM A213.
Chemical Composition of JIS G3463 SUS436LTB
For SUS436LTB, the melt ticket has to show Table 3 compliance — C ≤0.025, Si ≤1.00, Mn ≤1.00, P ≤0.040, S ≤0.030, Cr 16.00–19.00, Mo 0.75–1.25. Optional alloying footnotes in the standard still forbid blurring grade identity. Corrosion framing: Mo + stabilisation lifts pitting resistance in many waters vs 430LX. Every ladle analysis for SUS436LTB is checked against those windows before the heat is released to piercing, welding, or finishing, and the same numbers reappear on the inspection document. Corrosion framing beside SUS436LTB: Mo + stabilisation lifts pitting resistance in many waters vs 430LX.
Where Mo, Cu, Ti, Nb or N appear, they are intentional levers for SUS436LTB, not optional marketing. Confirm them on the MTC line-by-line. Role: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. If a purchaser specification tightens phosphorus, sulphur, or residual elements beyond Table 3, SHH STEEL will confirm melt feasibility for SUS436LTB before the order is acknowledged. Corrosion framing beside SUS436LTB: Mo + stabilisation lifts pitting resistance in many waters vs 430LX.
| Grade | C | Si | Mn | P | S | Cr | Mo | Ti/Nb/Zr |
|---|---|---|---|---|---|---|---|---|
| SUS436LTB | ≤0.025 | ≤1.00 | ≤1.00 | ≤0.040 | ≤0.030 | 16.00–19.00 | 0.75–1.25 | 8×(C%+N%)–0.80 |
Mechanical Properties of JIS G3463 SUS436LTB
Do not confuse Table 4 tube tensile floors with plate or tube standards that share the 436L Mo ferritic alias. For SUS436LTB under G3463 expect Rm min 410 N/mm², proof stress min 245 N/mm², elongation min 20% (OD ≥20 mm, No.11/12), verified per heat/lot rules in tensile sampling clauses. Tensile sampling follows tensile sampling clauses for the ordered test unit of SUS436LTB, and retests follow retest clauses when a result sits under the Table 4 floor. This paragraph is locked to SUS436LTB duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube.
| Grade | Rm min (N/mm²) | Proof stress min (N/mm²) | A OD≥20 mm No.11/12 min (%) | A 10≤OD<20 mm No.11 min (%) | A OD<10 mm No.11 min (%) |
|---|---|---|---|---|---|
| SUS436LTB | 410 | 245 | 20 | 15 | 12 |
Ambient values from JIS G3463 Table 4 for SUS436LTB. Heat treatment (Table 2): 720 °C min, air or slow cool. Elongation reductions apply for walls under 8 mm on No.12 pieces. For heat-exchanger tube the purchaser may designate an upper tensile limit (Table 4 min + 200 N/mm²) when necessary.
Manufacture of JIS G3463 SUS436LTB Tube (Seamless and Welded)
SHH STEEL can produce SUS436LTB as seamless S or as A/L/E welded tube, then heat-treat and pickle (or bright-anneal) per Table 2. Bevel ends are available by agreement; plain ends are the default when the PO is silent. Seamless and welded options remain available for SUS436LTB; the acknowledgement repeats the Table 1 symbols so production cannot silently change route after the PO is firm. Size practice for SUS436LTB remains HX OD in standard practice; confirm Mo on MTC.
Welded SUS436LTB needs weld-bead work or as-welded finish called out (as-welded vs cold-finished welded) so NDT and corrosion expectations match. Heat treatment: 720 °C min, air or slow cool. Ferritic heats are annealed (700 °C min, or 720 °C min for SUS430J1LTB) with rapid or slow cooling as Table 2 allows — not austenitic solution practice.
Hydrostatic testing or NDT (eddy current / ultrasonic per JIS G 0582/0583) replaces or accompanies pressure proof as the order states. Manufacture stays honest to the seamless or A/L/E welded choice. Size: HX OD in standard practice; confirm Mo on MTC. Hydrostatic pressure or NDT class for SUS436LTB is frozen with the size list so quality planners can book the correct benches before the tube is cut to length. This paragraph is locked to SUS436LTB duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube.
Dimensions and Tolerances for JIS G3463 SUS436LTB
Out-of-table OD×wall combinations are by agreement — still under the same grade symbol SUS436LTB. Duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. Tolerance class follows the process route ordered for SUS436LTB, and out-of-table diameters are accepted only with a written dimensional agreement on the same acknowledgement. This paragraph is locked to SUS436LTB duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube.
Ovality, wall eccentricity (where applicable), and weld bead height limits are part of dimensional tolerance clauses — not optional cosmetics. Size reminder: HX OD in standard practice; confirm Mo on MTC. Fixed lengths and multiple cut lengths for SUS436LTB are protected at the ends so bevel geometry and ID cleanliness survive inland and ocean transit. This paragraph is locked to SUS436LTB duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube.
Equivalent Grades for JIS G3463 SUS436LTB
SUS436LTB sits in JIS G3463 as a Mo-bearing stabilised ferritic heat-exchanger tube grade, giving a pitting step up from plain 430 without jumping into austenitic nickel cost. Body-only alias “436L Mo ferritic” is useful when buyers dual-cert talk against wrought SUS436L practice, but the governing HX tube mark remains SUS436LTB. Mo band on this pack was cross-checked to wrought SUS436L; confirm against paid G3463:2023 Table 3 before locking legal MTC language.
| System | Designation | Notes |
|---|---|---|
| JIS G3463 | SUS436LTB | Governing HX/boiler tube grade for this page |
| Commercial / UNS (body only) | 436L / Mo ferritic (UNS S43600 class talk) | Useful in dual-cert talk; confirm Mo on the cast line |
| ASTM A213 / A268 related | 436-family ferritic tube practice (no single TP asserted here) | Related chemistry family — different product standard; not interchangeable by default |
| EN / other | No one-to-one asserted | Starting point only; severe chlorides may need 444 or austenitic/duplex |
It is still ferritic — toughness and temperature limits apply. Compare SUS444TB, SUS430J1LTB, SUS430LXTB when Mo needs to rise further, or SUS316LTB when an austenitic route is justified. Hub: JIS G3463.
Heat Treatment and Delivery Condition for JIS G3463 SUS436LTB
Hot-finished seamless austenitics may use in-line rapid cool in lieu of a separate solution treatment under Table 2 note (a) unless the purchaser forbids it. Confirm for SUS436LTB. Band: 720 °C min, air or slow cool. Recorded furnace charts for SUS436LTB should support the Table 2 temperature claim on the certificate, including quench or cool method where the family requires rapid cooling. Keep the SUS436LTB caution visible here: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex.
Grain-size testing applies where the standard requires it for specific H grades — state any extra metallographic demand on the PO for SUS436LTB. Field heat treatment of SUS436LTB after hot bending must chase the same family practice, or the corrosion file should formally accept the as-bent condition. Keep the SUS436LTB caution visible here: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex.
Corrosion Resistance of JIS G3463 SUS436LTB
Medium, temperature, crevice geometry and weld condition decide whether SUS436LTB is enough. Summary: Mo + stabilisation lifts pitting resistance in many waters vs 430LX. Escalate via sisters SUS444TB, SUS430J1LTB, SUS430LXTB, SUS316LTB when coupons fail. Coupon orientation, weld condition, and surface finish for SUS436LTB belong in the corrosion test order so annex results can be compared to the installed bundle honestly. Size practice for SUS436LTB remains HX OD in standard practice; confirm Mo on MTC.
Surface finish and iron contamination control often matter as much as bulk chemistry on sanitary-lean duties for SUS436LTB. Corrosion framing: Mo + stabilisation lifts pitting resistance in many waters vs 430LX. If operating chlorides, temperature, or crevice geometry change after award, reopen the alloy choice for SUS436LTB rather than relying on schedule thickness alone. Weld-shop note tied to SUS436LTB: 436L/stabilised Mo ferritic fillers; low heat input.
Applications of JIS G3463 SUS436LTB Tube
From utility rooms to process racks, SUS436LTB shows up wherever Japanese boiler/HX specs want ferritic behaviour. Use list: mild chloride coolers, automotive-adjacent exchangers, and ferritic HX needing a Mo bump. Spool fabricators should copy SUS436LTB onto cut lists and WPS bases so warehouse substitutions cannot quietly introduce a different carbon or molybdenum window. Corrosion framing beside SUS436LTB: Mo + stabilisation lifts pitting resistance in many waters vs 430LX.
If the only reason for SUS436LTB is “we always used this alias,” reopen the corrosion file before repeating the order. Caution: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex. Commissioning teams benefit when the as-built dossier repeats SUS436LTB beside heat numbers, linking isometric revisions to the same mill certificates. Weld-shop note tied to SUS436LTB: 436L/stabilised Mo ferritic fillers; low heat input.
Weldability of JIS G3463 SUS436LTB
Automatic mill welds and manual field welds need different procedure packs, but both must respect SUS436LTB chemistry. Guidance: 436L/stabilised Mo ferritic fillers; low heat input. Procedure qualification for SUS436LTB should use the same product form and wall class as production, including any bead-worked or as-welded finish that will ship. This paragraph is locked to SUS436LTB duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube.
Ferrite control on duplex SUS436LTB and hot-crack control on high-Ni austenitics are procedure items, not afterthoughts. Guidance: 436L/stabilised Mo ferritic fillers; low heat input. Consumable lot control and shielding-gas notes for SUS436LTB stay with the WPS package so site crews cannot improvise fillers that under-alloy the joint. This paragraph is locked to SUS436LTB duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube.
Surface Finishes for JIS G3463 SUS436LTB
Mild-chloride coolers and automotive-adjacent exchangers in SUS436LTB usually ship annealed and pickled after heat treatment, with Mo already verified on the MTC before finish talk starts. Bright anneal covers scale-free OD/ID appearance orders; ground or polished finishes are by agreement when the RFQ names a roughness. Welded routes may need bead dressing for flow or inspection — call that out rather than assuming mill habit on this Mo ferritic.
| Finish | Typical supply | Order note |
|---|---|---|
| Annealed and pickled | Standard HX mill finish after anneal | Matte, scale-free; Mo confirmed on MTC |
| Bright annealed | Scale-free OD/ID when ordered | State OD, ID, or both |
| Ground / polished / bead dressed | By agreement for roughness or weld flush | Name Ra/grit and surface; inspect before polish |
| Passivated | When chloride-lean end-user specs require it | Not a substitute for anneal or Mo chemistry control |
Passivation helps after pickling or shop welding, but it will not fix a missed anneal or a cast that missed the Mo window. Keep free-iron contamination and chloride-bearing packing films off finished SUS436LTB bundles; ferritic Mo grades still stain if carbon-steel tooling marks the OD.
Inspection and Testing for JIS G3463 SUS436LTB
Third-party witness (SGS/TUV-style) is available when the project mandate requires it. Base acceptance still tracks G3463 for SUS436LTB. Sampling plans for SUS436LTB keep heat identity unbroken from melt through bundle tags, including any third-party hold points written into the purchase order. Application context for SUS436LTB stays mild chloride coolers, automotive-adjacent exchangers, and ferritic HX needing a Mo bump.
Dimensional inspection against dimensional tolerance clauses tolerances closes the lot. Failures retest per retest clauses — they are not silently shipped. Role: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. Non-conforming SUS436LTB lengths are segregated and retested or rejected under retest clauses rather than reworked into unmarked stock. Keep the SUS436LTB caution visible here: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex.
Packaging and Shipping for JIS G3463 SUS436LTB
Seaworthy packing is available for ocean legs — desiccant, VCI, and wrap specs by agreement. Grade mark SUS436LTB stays visible on outer tags. Bundle tickets for SUS436LTB repeat grade, heat, size, and quantity so receiving inspectors can match crates to the packing list without opening every wrap. Size practice for SUS436LTB remains HX OD in standard practice; confirm Mo on MTC.
Container loading plans should keep heavy schedules from crushing thin-wall SUS436LTB layers. Desiccant and wrap choices for SUS436LTB follow the voyage length and storage climate stated on the shipping order, not a one-size export habit. Application context for SUS436LTB stays mild chloride coolers, automotive-adjacent exchangers, and ferritic HX needing a Mo bump.
Shortages or transit damage claims need photos against the packing list before installation starts — tag identity must still read SUS436LTB. Claims handling for SUS436LTB starts with tagged photos against the packing list so heat identity remains usable if replacement lengths are required. Corrosion framing beside SUS436LTB: Mo + stabilisation lifts pitting resistance in many waters vs 430LX.
Why Choose SHH STEEL
From RFQ clarification through MTC release, SHH STEEL treats SUS436LTB as a governed product symbol, not a marketing synonym for 436L Mo ferritic. Role: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. SHH STEEL can produce and supply SUS436LTB against the OD × wall, process symbol, and test scope on your RFQ without swapping in an unstated sister grade.
Response time stays short because common SUS436LTB enquiry sizes and document packs are already exercised on prior Japanese-spec orders. Use: mild chloride coolers, automotive-adjacent exchangers, and ferritic HX needing a Mo bump. Ask for a written acknowledgement that names SUS436LTB, the manufacture process/finish marks, and the Table 2 heat-treatment condition before melt. SHH STEEL can make SUS436LTB to that written scope.
Supply Capability
Capability framing for SUS436LTB: Japanese-spec HX tube product, dual-route manufacture, documented heats. Caution remains: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex. SHH STEEL can produce and supply cut lengths, bevels, and ordered annex tests for SUS436LTB when the mill schedule allows. SHH STEEL can produce and supply cut lengths, bevels, and ordered annex tests for SUS436LTB when the mill schedule allows. Weld-shop note tied to SUS436LTB: 436L/stabilised Mo ferritic fillers; low heat input.
| Item | Capability |
|---|---|
| Standard | JIS G3463 stainless steel tubes for boilers and heat exchangers |
| Grade symbol | SUS436LTB |
| Product form | Seamless (S) and welded (A / L / E) tube; finishes S-H / S-C / A / A-C / E-C as marked |
| Delivery condition | annealed |
| Documents | Mill test certificate (JIS G 0415 / EN 10204 3.1 style as ordered) |
| Typical OD practice | 15.9–139.8 mm per standard Note 1; other by agreement |
| Wall / gauge | OD × wall / BWG-class HX gauges within Attached Tables; other by agreement |
Stock / Available sizes
Stock / Available sizes — treat published ranges as capability envelopes. Actual ex-stock pieces of SUS436LTB change weekly; the reliable path is an OD × wall matrix on the enquiry. Duty: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. SHH STEEL can supply alternate schedules and measured walls for SUS436LTB once the design pressure and corrosion allowance are clear.
Repeat orders for SUS436LTB go faster when prior heat records and accepted WPS numbers are referenced on the new RFQ. Role: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. SHH STEEL can produce trial lengths of SUS436LTB for procedure qualification before the bulk release when the project calendar needs it.
FAQ
-
What is JIS G3463 SUS436LTB stainless steel tube used for?
- JIS G3463 SUS436LTB is stainless tube for boiler and heat-exchanger service (superheater, HX, condenser, catalyser) — mild chloride coolers, automotive-adjacent exchangers, and ferritic HX needing a Mo bump. Role summary: Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. It is a Japanese boiler/HX tube product standard mark, not an automatic ASTM A213 certificate.
-
Does JIS G3463 SUS436LTB cover seamless and welded tube?
- Yes. Manufacture allows seamless and welded automatic-arc (A), laser (L), or electric-resistance (E) routes with finish marks such as S-H, S-C, A-C, or E-C. SHH STEEL can produce and supply either route for SUS436LTB when the mill can meet the ordered size and tests. The title omits Seamless/Welded because JIS G3463 covers both manufacture routes — the PO must still name the process mark.
-
What heat treatment applies to SUS436LTB?
- SUS436LTB is delivered annealed under JIS G3463. Table 2 reference: 720 °C min, air or slow cool. Stabilisation or other purchaser options, where allowed, must be written on the order. Certificate wording should match the treatment actually performed.
-
How does SUS436LTB compare with sister grades SUS444TB, SUS430J1LTB, SUS430LXTB?
- SUS436LTB is filed as ferritic. Typical sisters on the same RFQ are SUS444TB, SUS430J1LTB, SUS430LXTB. Design caution: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex Pick the sister when the medium or strength floor outgrows this symbol rather than stretching wall alone.
-
What tests appear on the mill certificate for SUS436LTB?
- Expect cast analysis (Table 3), room-temperature tensile results (Table 4), flattening/flaring as applicable, dimensions, hydrostatic or NDT as ordered, and every special annex test actually performed. SHH STEEL does not print surrogate inspection lines. Documents follow JIS G 0415 or EN 10204 3.1 style when specified.
-
Is 436L Mo ferritic the same as ordering SUS436LTB?
- No. 436L Mo ferritic is a commercial / UNS cross-walk for body text. The purchase order should lock JIS G3463 and SUS436LTB so cast limits, heat treatment, and process marks are unambiguous. Silent alias substitution is a common root cause of wrong MTCs.
-
What size range can SHH STEEL quote for JIS G3463 SUS436LTB?
- SHH STEEL can produce and supply enquiry-oriented OD × wall bands for SUS436LTB within the typical 15.9–139.8 mm OD practice, with measured walls by agreement. Size context: HX OD in standard practice; confirm Mo on MTC. Stock / Available sizes on this page is an RFQ map, not a frozen tonnage catalogue.
-
How should SUS436LTB be welded?
- Shop guidance: 436L/stabilised Mo ferritic fillers; low heat input. Mill heat treatment of seamless or welded tube does not replace a qualified WPS on fabricator joints or tube-to-tubesheet welds. For corrosive as-welded duty, confirm low-carbon, stabilisation, duplex ferrite control, or anneal practice as applicable. Caution: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex
-
When should I choose a duplex or higher-Mo grade instead of SUS436LTB?
- Move when chloride pitting, crevice attack, or SCC risk exceeds what ferritic practice can defend for the temperature and stress state. Caution for this mark: still ferritic — toughness and temperature limits apply; severe chlorides may need 444 or austenitic/duplex Sister pointers: SUS444TB, SUS430J1LTB, SUS430LXTB. SHH STEEL will not invent PREN marketing digits — bring the medium data.
-
Can SHH STEEL dual-certify JIS G3463 SUS436LTB with ASTM A213 or ASME SA213?
- Dual documentation is possible only when chemistry and tests satisfy each standard on its own terms. An MTC that only cites JIS G3463 SUS436LTB does not clear ASTM A213 acceptance by default. State both standards, sizes, and test scopes before melt.
-
What surface finishes are available for SUS436LTB?
- Pickled after heat treatment is the usual HX tube supply. Bright anneal, grind, or polish finishes are by agreement and must state OD/ID scope. SHH STEEL can produce and supply the ordered finish for SUS436LTB when the mill route supports it. Carbon-steel strapping never contacts the stainless OD.
Conclusion
JIS G3463 SUS436LTB is stainless steel tube for boiler and heat-exchanger service — Mo-bearing stabilised ferritic for better pitting resistance than plain 430 in HX tube. SHH STEEL can produce and supply it in seamless or welded routes with the heat treatment, tests, and finishes named on your enquiry, documented on mill certificates. Sister grades often discussed alongside this mark include SUS444TB, SUS430J1LTB, SUS430LXTB. Related ASTM A213 pages share chemistry families but not Japanese acceptance text. Email admin@steelspecs.com with OD × wall, process mark, and medium notes to start the quote.