JIS G3463 SUS405TB Stainless Steel Tube
What is JIS G3463 SUS405TB Stainless Steel Tube
JIS G3463 covers both seamless and welded stainless tube for process, utility, condenser and heat-exchange duties. Inside that standard, SUS405TB is filed as ferritic. JIS G3463 SUS405TB is a ferritic HX choice for mild service — do not order it hoping for 304-class chloride performance. Buyers working Japanese boiler and HX packages should treat SUS405TB as a governed product symbol under G3463, with Table 3 chemistry and Table 4 tensile floors enforced on the same heat. This paragraph is locked to SUS405TB duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube.
From pierce/draw or weld-and-anneal through marking and bundle protection, SHH STEEL can produce JIS G3463 SUS405TB for the sizes and tests on your RFQ. Application sketch: mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary. Size and test clarity on the RFQ lets SHH STEEL lock the correct Table 1 symbols for SUS405TB before production starts. This paragraph is locked to SUS405TB duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube.
On the floor people shorten marks; in QA they must not. SUS405TB under JIS G3463 carries specific Table 3 windows and Table 4 floors that a loose “405” note will not enforce. Caution: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty. Keep isometric notes, tubesheet specs, and the mill acknowledgement aligned on SUS405TB so informal alias language cannot reopen the carbon or molybdenum window after melt. This paragraph is locked to SUS405TB duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube.
Superheater, condenser and corrosive HX duties all sit in G3463’s scope statement; still match the alloy to the medium. For SUS405TB, that means: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. Nearby marks: SUS409TB, SUS410TB, SUS430TB, SUS409LTB. Document the medium, design temperature, and weld map beside the SUS405TB line item so sister-grade swaps are engineering decisions rather than purchasing shortcuts. This paragraph is locked to SUS405TB duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube.
Inside this JIS G3463 series, compare SUS409TB, SUS410TB, SUS430TB, SUS409LTB. Hub: JIS G3463. ASTM/ASME related product pages (not interchangeable by default): ASTM A213.
Chemical Composition of JIS G3463 SUS405TB
For SUS405TB, the melt ticket has to show Table 3 compliance — C ≤0.08, Si ≤1.00, Mn ≤1.00, P ≤0.040, S ≤0.030, Cr 11.50–14.50, Al 0.10–0.30. Optional alloying footnotes in the standard still forbid blurring grade identity. Corrosion framing: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics.
Where Mo, Cu, Ti, Nb or N appear, they are intentional levers for SUS405TB, not optional marketing. Confirm them on the MTC line-by-line. Role: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. If a purchaser specification tightens phosphorus, sulphur, or residual elements beyond Table 3, SHH STEEL will confirm melt feasibility for SUS405TB before the order is acknowledged. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials.
| Grade | C | Si | Mn | P | S | Cr | Al |
|---|---|---|---|---|---|---|---|
| SUS405TB | ≤0.08 | ≤1.00 | ≤1.00 | ≤0.040 | ≤0.030 | 11.50–14.50 | 0.10–0.30 |
Mechanical Properties of JIS G3463 SUS405TB
Do not confuse Table 4 tube tensile floors with plate or tube standards that share the 405 / UNS S40500 alias. For SUS405TB under G3463 expect Rm min 412 N/mm², proof stress min 206 N/mm², elongation min 20% (OD ≥20 mm, No.11/12), verified per heat/lot rules in tensile sampling clauses. Tensile sampling follows tensile sampling clauses for the ordered test unit of SUS405TB, and retests follow retest clauses when a result sits under the Table 4 floor. Application context for SUS405TB stays mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary.
| Grade | Rm min (N/mm²) | Proof stress min (N/mm²) | A OD≥20 mm No.11/12 min (%) | A 10≤OD<20 mm No.11 min (%) | A OD<10 mm No.11 min (%) |
|---|---|---|---|---|---|
| SUS405TB | 412 | 206 | 20 | 15 | 12 |
Ambient values from JIS G3463 Table 4 for SUS405TB. Heat treatment (Table 2): 700 °C min, air or slow cool. Elongation reductions apply for walls under 8 mm on No.12 pieces. For heat-exchanger tube the purchaser may designate an upper tensile limit (Table 4 min + 200 N/mm²) when necessary.
Manufacture of JIS G3463 SUS405TB Tube (Seamless and Welded)
SHH STEEL can produce SUS405TB as seamless S or as A/L/E welded tube, then heat-treat and pickle (or bright-anneal) per Table 2. Bevel ends are available by agreement; plain ends are the default when the PO is silent. Seamless and welded options remain available for SUS405TB; the acknowledgement repeats the Table 1 symbols so production cannot silently change route after the PO is firm. Application context for SUS405TB stays mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary.
Welded SUS405TB needs weld-bead work or as-welded finish called out (as-welded vs cold-finished welded) so NDT and corrosion expectations match. Heat treatment: 700 °C min, air or slow cool. Ferritic heats are annealed (700 °C min, or 720 °C min for SUS430J1LTB) with rapid or slow cooling as Table 2 allows — not austenitic solution practice.
Hydrostatic testing or NDT (eddy current / ultrasonic per JIS G 0582/0583) replaces or accompanies pressure proof as the order states. Manufacture stays honest to the seamless or A/L/E welded choice. Size: light HX walls; annealed delivery; avoid sharp U-bends without procedure trials. Hydrostatic pressure or NDT class for SUS405TB is frozen with the size list so quality planners can book the correct benches before the tube is cut to length. Weld-shop note tied to SUS405TB: ferritic practices; low heat input; matching or 410/405-class fillers per WPS.
Dimensions and Tolerances for JIS G3463 SUS405TB
Out-of-table OD×wall combinations are by agreement — still under the same grade symbol SUS405TB. Duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. Tolerance class follows the process route ordered for SUS405TB, and out-of-table diameters are accepted only with a written dimensional agreement on the same acknowledgement. Keep the SUS405TB caution visible here: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty.
Ovality, wall eccentricity (where applicable), and weld bead height limits are part of dimensional tolerance clauses — not optional cosmetics. Size reminder: light HX walls; annealed delivery; avoid sharp U-bends without procedure trials. Fixed lengths and multiple cut lengths for SUS405TB are protected at the ends so bevel geometry and ID cleanliness survive inland and ocean transit. Corrosion framing beside SUS405TB: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics.
Equivalent Grades for JIS G3463 SUS405TB
European EN tube/tube numbers and ASTM marks may sit near 405 / UNS S40500, yet hydrostatic, NDT and heat-treatment text diverge. Keep SUS405TB as the governing symbol unless a written dual-cert plan exists. Caution: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty. When a dual-cert path is required, list both JIS G3463 SUS405TB and the ASTM mark with separate test scopes instead of assuming one chemistry line clears both files. This paragraph is locked to SUS405TB duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube.
Heat Treatment and Delivery Condition for JIS G3463 SUS405TB
Hot-finished seamless austenitics may use in-line rapid cool in lieu of a separate solution treatment under Table 2 note (a) unless the purchaser forbids it. Confirm for SUS405TB. Band: 700 °C min, air or slow cool. Recorded furnace charts for SUS405TB should support the Table 2 temperature claim on the certificate, including quench or cool method where the family requires rapid cooling. Keep the SUS405TB caution visible here: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty.
Grain-size testing applies where the standard requires it for specific H grades — state any extra metallographic demand on the PO for SUS405TB. Field heat treatment of SUS405TB after hot bending must chase the same family practice, or the corrosion file should formally accept the as-bent condition. Corrosion framing beside SUS405TB: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics.
Corrosion Resistance of JIS G3463 SUS405TB
Medium, temperature, crevice geometry and weld condition decide whether SUS405TB is enough. Summary: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics. Escalate via sisters SUS409TB, SUS410TB, SUS430TB, SUS409LTB when coupons fail. Coupon orientation, weld condition, and surface finish for SUS405TB belong in the corrosion test order so annex results can be compared to the installed bundle honestly. Application context for SUS405TB stays mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary.
Surface finish and iron contamination control often matter as much as bulk chemistry on sanitary-lean duties for SUS405TB. Corrosion framing: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics. If operating chlorides, temperature, or crevice geometry change after award, reopen the alloy choice for SUS405TB rather than relying on schedule thickness alone. This paragraph is locked to SUS405TB duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube.
Applications of JIS G3463 SUS405TB Tube
From utility rooms to process racks, SUS405TB shows up wherever Japanese boiler/HX specs want ferritic behaviour. Use list: mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary. Spool fabricators should copy SUS405TB onto cut lists and WPS bases so warehouse substitutions cannot quietly introduce a different carbon or molybdenum window. Weld-shop note tied to SUS405TB: ferritic practices; low heat input; matching or 410/405-class fillers per WPS.
If the only reason for SUS405TB is “we always used this alias,” reopen the corrosion file before repeating the order. Caution: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty. Commissioning teams benefit when the as-built dossier repeats SUS405TB beside heat numbers, linking isometric revisions to the same mill certificates. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials.
Weldability of JIS G3463 SUS405TB
Automatic mill welds and manual field welds need different procedure packs, but both must respect SUS405TB chemistry. Guidance: ferritic practices; low heat input; matching or 410/405-class fillers per WPS. Procedure qualification for SUS405TB should use the same product form and wall class as production, including any bead-worked or as-welded finish that will ship. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials.
Ferrite control on duplex SUS405TB and hot-crack control on high-Ni austenitics are procedure items, not afterthoughts. Guidance: ferritic practices; low heat input; matching or 410/405-class fillers per WPS. Consumable lot control and shielding-gas notes for SUS405TB stay with the WPS package so site crews cannot improvise fillers that under-alloy the joint. Corrosion framing beside SUS405TB: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics.
Surface Finishes for JIS G3463 SUS405TB
Welded tube may need bead dressing for flow or inspection; call that out rather than assuming mill habit. Size/finish context: light HX walls; annealed delivery; avoid sharp U-bends without procedure trials. Roughness or polish callouts for SUS405TB must name OD, ID, or both; ambiguous “bright tube” language is clarified before finishing slots are booked. Corrosion framing beside SUS405TB: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics.
Do not polish over unresolved weld defects — inspection comes before cosmetics on SUS405TB. Final visual standards for SUS405TB reject grinding burns, embedded free iron, and unrepaired weld undercut before bundles are closed. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials Final visual standards for SUS405TB reject grinding burns, embedded free iron, and unrepaired weld undercut before bundles are closed. Order-line discipline for SUS405TB still points at role: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube.
Inspection and Testing for JIS G3463 SUS405TB
Third-party witness (SGS/TUV-style) is available when the project mandate requires it. Base acceptance still tracks G3463 for SUS405TB. Sampling plans for SUS405TB keep heat identity unbroken from melt through bundle tags, including any third-party hold points written into the purchase order. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials.
Dimensional inspection against dimensional tolerance clauses tolerances closes the lot. Failures retest per retest clauses — they are not silently shipped. Role: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. Non-conforming SUS405TB lengths are segregated and retested or rejected under retest clauses rather than reworked into unmarked stock. Corrosion framing beside SUS405TB: 12Cr + Al handles mild aqueous and some heat-adjacent duties; pitting resistance trails Mo austenitics.
Packaging and Shipping for JIS G3463 SUS405TB
Seaworthy packing is available for ocean legs — desiccant, VCI, and wrap specs by agreement. Grade mark SUS405TB stays visible on outer tags. Bundle tickets for SUS405TB repeat grade, heat, size, and quantity so receiving inspectors can match crates to the packing list without opening every wrap. Application context for SUS405TB stays mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary.
Container loading plans should keep heavy schedules from crushing thin-wall SUS405TB layers. Desiccant and wrap choices for SUS405TB follow the voyage length and storage climate stated on the shipping order, not a one-size export habit. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials Desiccant and wrap choices for SUS405TB follow the voyage length and storage climate stated on the shipping order, not a one-size export habit. Use-case reminder for SUS405TB: mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary.
Shortages or transit damage claims need photos against the packing list before installation starts — tag identity must still read SUS405TB. Claims handling for SUS405TB starts with tagged photos against the packing list so heat identity remains usable if replacement lengths are required. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials.
Why Choose SHH STEEL
From RFQ clarification through MTC release, SHH STEEL treats SUS405TB as a governed product symbol, not a marketing synonym for 405 / UNS S40500. Role: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. SHH STEEL can produce and supply SUS405TB against the OD × wall, process symbol, and test scope on your RFQ without swapping in an unstated sister grade.
Response time stays short because common SUS405TB enquiry sizes and document packs are already exercised on prior Japanese-spec orders. Use: mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary. Ask for a written acknowledgement that names SUS405TB, the manufacture process/finish marks, and the Table 2 heat-treatment condition before melt. SHH STEEL can make SUS405TB to that written scope.
Supply Capability
Capability framing for SUS405TB: Japanese-spec HX tube product, dual-route manufacture, documented heats. Caution remains: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty. SHH STEEL can produce and supply cut lengths, bevels, and ordered annex tests for SUS405TB when the mill schedule allows. SHH STEEL can produce and supply cut lengths, bevels, and ordered annex tests for SUS405TB when the mill schedule allows. Size practice for SUS405TB remains light HX walls; annealed delivery; avoid sharp U-bends without procedure trials.
| Item | Capability |
|---|---|
| Standard | JIS G3463 stainless steel tubes for boilers and heat exchangers |
| Grade symbol | SUS405TB |
| Product form | Seamless (S) and welded (A / L / E) tube; finishes S-H / S-C / A / A-C / E-C as marked |
| Delivery condition | annealed |
| Documents | Mill test certificate (JIS G 0415 / EN 10204 3.1 style as ordered) |
| Typical OD practice | 15.9–139.8 mm per standard Note 1; other by agreement |
| Wall / gauge | OD × wall / BWG-class HX gauges within Attached Tables; other by agreement |
Stock / Available sizes
Stock / Available sizes — treat published ranges as capability envelopes. Actual ex-stock pieces of SUS405TB change weekly; the reliable path is an OD × wall matrix on the enquiry. Duty: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. SHH STEEL can supply alternate schedules and measured walls for SUS405TB once the design pressure and corrosion allowance are clear.
Repeat orders for SUS405TB go faster when prior heat records and accepted WPS numbers are referenced on the new RFQ. Role: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. SHH STEEL can produce trial lengths of SUS405TB for procedure qualification before the bulk release when the project calendar needs it.
FAQ
-
What is JIS G3463 SUS405TB stainless steel tube used for?
- JIS G3463 SUS405TB is stainless tube for boiler and heat-exchanger service (superheater, HX, condenser, catalyser) — mild water coolers, heat-adjacent utility exchangers, and low-cost ferritic HX where austenitic is unnecessary. Role summary: Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. It is a Japanese boiler/HX tube product standard mark, not an automatic ASTM A213 certificate.
-
Does JIS G3463 SUS405TB cover seamless and welded tube?
- Yes. Manufacture allows seamless and welded automatic-arc (A), laser (L), or electric-resistance (E) routes with finish marks such as S-H, S-C, A-C, or E-C. SHH STEEL can produce and supply either route for SUS405TB when the mill can meet the ordered size and tests. The title omits Seamless/Welded because JIS G3463 covers both manufacture routes — the PO must still name the process mark.
-
What heat treatment applies to SUS405TB?
- SUS405TB is delivered annealed under JIS G3463. Table 2 reference: 700 °C min, air or slow cool. Stabilisation or other purchaser options, where allowed, must be written on the order. Certificate wording should match the treatment actually performed.
-
How does SUS405TB compare with sister grades SUS409TB, SUS410TB, SUS430TB?
- SUS405TB is filed as ferritic. Typical sisters on the same RFQ are SUS409TB, SUS410TB, SUS430TB. Design caution: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty Pick the sister when the medium or strength floor outgrows this symbol rather than stretching wall alone.
-
What tests appear on the mill certificate for SUS405TB?
- Expect cast analysis (Table 3), room-temperature tensile results (Table 4), flattening/flaring as applicable, dimensions, hydrostatic or NDT as ordered, and every special annex test actually performed. SHH STEEL does not print surrogate inspection lines. Documents follow JIS G 0415 or EN 10204 3.1 style when specified.
-
Is 405 / UNS S40500 the same as ordering SUS405TB?
- No. 405 / UNS S40500 is a commercial / UNS cross-walk for body text. The purchase order should lock JIS G3463 and SUS405TB so cast limits, heat treatment, and process marks are unambiguous. Silent alias substitution is a common root cause of wrong MTCs.
-
What size range can SHH STEEL quote for JIS G3463 SUS405TB?
- SHH STEEL can produce and supply enquiry-oriented OD × wall bands for SUS405TB within the typical 15.9–139.8 mm OD practice, with measured walls by agreement. Size context: light HX walls; annealed delivery; avoid sharp U-bends without procedure trials. Stock / Available sizes on this page is an RFQ map, not a frozen tonnage catalogue.
-
How should SUS405TB be welded?
- Shop guidance: ferritic practices; low heat input; matching or 410/405-class fillers per WPS. Mill heat treatment of seamless or welded tube does not replace a qualified WPS on fabricator joints or tube-to-tubesheet welds. For corrosive as-welded duty, confirm low-carbon, stabilisation, duplex ferrite control, or anneal practice as applicable. Caution: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty
-
When should I choose a duplex or higher-Mo grade instead of SUS405TB?
- Move when chloride pitting, crevice attack, or SCC risk exceeds what ferritic practice can defend for the temperature and stress state. Caution for this mark: ferritic toughness and weld grain growth limits apply — not for cryogenic or severe chloride duty Sister pointers: SUS409TB, SUS410TB, SUS430TB. SHH STEEL will not invent PREN marketing digits — bring the medium data.
-
Can SHH STEEL dual-certify JIS G3463 SUS405TB with ASTM A213 or ASME SA213?
- Dual documentation is possible only when chemistry and tests satisfy each standard on its own terms. An MTC that only cites JIS G3463 SUS405TB does not clear ASTM A213 acceptance by default. State both standards, sizes, and test scopes before melt.
-
What surface finishes are available for SUS405TB?
- Pickled after heat treatment is the usual HX tube supply. Bright anneal, grind, or polish finishes are by agreement and must state OD/ID scope. SHH STEEL can produce and supply the ordered finish for SUS405TB when the mill route supports it. Carbon-steel strapping never contacts the stainless OD.
Conclusion
JIS G3463 SUS405TB is stainless steel tube for boiler and heat-exchanger service — Al-bearing 12Cr ferritic for mild aqueous and heat-adjacent HX tube. SHH STEEL can produce and supply it in seamless or welded routes with the heat treatment, tests, and finishes named on your enquiry, documented on mill certificates. Sister grades often discussed alongside this mark include SUS409TB, SUS410TB, SUS430TB. Related ASTM A213 pages share chemistry families but not Japanese acceptance text. Email admin@steelspecs.com with OD × wall, process mark, and medium notes to start the quote.