ASTM A312 UNS S31272 Stainless Steel Pipe | ASTM A312 Stainless Steel - SHH STEEL

ASTM A312 UNS S31272 Stainless Steel Pipe

ASTM A312 UNS S31272 titanium-boron stabilized 15Cr-15Ni-Mo stainless steel pipe in SML, WLD and HCW, with a Table 4 floor of 65/29 ksi and a 1920 °F [1050 °C] minimum anneal, supplied by SHH STEEL to B36.19 or special sizes with EN 10204 3.1 MTCs.
Grade
UNS S31272
Standard
ASTM A312 / A312M
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASTM A312 UNS S31272 Stainless Steel Pipe

ASTM A312/A312M is the ASTM product specification for seamless, welded and heavily cold-worked austenitic stainless steel pipe intended for high-temperature and general corrosive service. It is a standard in its own right, maintained by ASTM, and this page is written against A312/A312M for UNS S31272, with every number taken from the A312 tables. ASME publishes a separate Code standard, SA-312, which is a different document even where its text runs parallel, so the two titles should not be treated as synonyms on a purchase order.

Within A312, UNS S31272 is a titanium-boron stabilized 15Cr-15Ni-Mo grade listed by UNS number only, with no TP designation. Table 1 sets C 0.08–0.12%, Mn 1.5–2.0%, Si 0.25–0.75%, Cr 14.0–16.0%, Ni 14.0–16.0%, Mo 1.00–1.40%, Ti 0.30–0.60% and B 0.004–0.008%. Table 4 requires 65 ksi [450 MPa] tensile and 29 ksi [200 MPa] yield, with elongation of 35% longitudinal / 25% transverse (general austenitic rule), and Table 2 calls for a solution anneal at 1920 °F [1050 °C] minimum followed by rapid cooling. Table 2 lists S31272 with S30815 at this temperature, slightly above the 1900 °F [1040 °C] default, so a habitual 316 anneal is not automatic compliance.

S31272 is an unusual grade in A312 because its chemistry is designed for elevated-temperature stability rather than chloride resistance. Carbon is a required band of 0.08–0.12%, not a maximum, and it is balanced by titanium at 0.30–0.60% and a very small, controlled boron addition of 0.004–0.008%. Chromium and nickel are both 14.0–16.0%, with 1.00–1.40% molybdenum, so the alloy is leaner than 316 in Cr but richer in Ni.

That combination of a carbon floor, titanium carbonitrides and boron is a familiar recipe for creep strength in austenitic steel. The Table 4 row is modest at room temperature, 65 ksi [450 MPa] tensile and 29 ksi [200 MPa] yield, which reminds buyers that this grade is not specified for ambient strength. It appears on owner grade lists for specialty high-temperature process lines and engineered substitutions, and should only be ordered when the datasheet actually names it.

SHH STEEL can supply ASTM A312 UNS S31272 stainless steel pipe as seamless (SML), welded (WLD) or heavily cold-worked (HCW) product, in ASME B36.19 schedules or special OD and wall combinations, with EN 10204 3.1 mill test certificates showing the full Table 1 analysis, the Table 4 results and the anneal actually applied. Third-party 3.2 inspection is arranged when the enquiry names the agency. If a project also needs ASME SA-312 marking for Code piping, we arrange dual marking only when the purchase order asks for it; the separate ASME-framed page for this grade is SA312 UNS S31272.

In the market this chemistry may appear as the informal “15-15Ti” label; there is no TP designation and no reliable EN equivalent to quote. Those labels are useful in conversation but carry no acceptance value; the pipe is UNS S31272 only when the heat certificate matches Table 1 line by line. Buyers comparing options within the ASTM series usually look next at A312 UNS S35045, A312 UNS S35315, A312 TP316Ti, A312 TP321 and A312 TP316H, and the full grade list sits on the A312/A312M hub. None of those pages describes a drop-in substitute, because chemistry, strength and anneal differ in ways that matter to the design.

Manufacturing Types (SML / WLD / HCW)

A312 recognizes three manufacturing routes for UNS S31272 pipe, and choosing between them is a purchase-order decision based on the design code, the size and wall, and how the owner wants the pipe inspected. The route never relaxes the chemistry: whichever way the pipe is made, the heat must still meet Table 1 and every length must still be solution annealed at 1920 °F [1050 °C] minimum before release.

  • Seamless (SML) — made without welding at any stage. It is usually preferred for heavy walls, high-pressure lines and owners who exclude welded pipe from a design class, and it is the common route for small-bore UNS S31272 lines.
  • Welded (WLD) — made from strip or plate by an automatic process without filler metal in the longitudinal seam, then heat treated. The strip or plate heat must itself carry the full UNS S31272 chemistry, so the certificate should trace the coil or plate heat number.
  • Heavily cold-worked (HCW) — welded pipe cold worked by at least 35% reduction of wall and weld before the final anneal, with the weld radiographed before cold working. Order it only when the project specifically calls for the HCW marking and its process controls.

Every finished length is either hydrostatically tested or tested by a nondestructive electric method, and the mill may choose unless the purchase order fixes one. Mechanical test lots follow the sampling clauses of the referenced A312 edition. Naming SML, WLD or HCW on the enquiry lets the mill line up material, heat treatment and test plans before the heat is allocated, which is especially important for a UNS-only grade like UNS S31272 that is rarely held as general stock.

Chemical Composition of ASTM A312 UNS S31272

Two layers of chemistry apply to ASTM A312 UNS S31272. The melting (heat) analysis in Table 1 is mandatory on every heat and is the figure the mill reports on the certificate. Product analysis on finished pipe is optional; when Supplementary Requirement S1 is ordered, the A480/A480M Annex A1.1 tolerances define how far a check analysis may deviate from the Table 1 limits.

The first table shows the Table 1 melting limits. Read single values as maximums and ranges as both a floor and a ceiling, and expect every element in the table to appear on the MTC as a measured value rather than a summary line.

Element UNS S31272 melting analysis
Carbon (C) 0.08 – 0.12
Manganese (Mn) 1.50 – 2.00
Phosphorus (P) ≤ 0.030
Sulfur (S) ≤ 0.015
Silicon (Si) 0.25 – 0.75
Chromium (Cr) 14.0 – 16.0
Nickel (Ni) 14.0 – 16.0
Molybdenum (Mo) 1.00 – 1.40
Titanium (Ti) 0.30 – 0.60
Boron (B) 0.004 – 0.008

For UNS S31272 the elements given as ranges deserve the closest look, because they define the grade rather than merely limit impurities. A heat that drifts outside any of those ranges is not UNS S31272, however close the rest of the analysis looks, and checking each range element against the certificate is the first job of receiving inspection.

When product analysis is ordered, the second table pairs each Table 1 limit with its A480 tolerance and the resulting acceptance limit on finished pipe. It lets an inspector judge a check-analysis result without reworking the tolerance rules by hand.

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) 0.08 – 0.12 0.01 under / over 0.07 – 0.13
Manganese (Mn) 1.50 – 2.00 0.04 under / over 1.46 – 2.04
Phosphorus (P) ≤ 0.030 0.005 over ≤ 0.035
Sulfur (S) ≤ 0.015 0.005 over ≤ 0.020
Silicon (Si) 0.25 – 0.75 0.05 under / over 0.20 – 0.80
Chromium (Cr) 14.0 – 16.0 0.15 under / over 13.85 – 16.15
Nickel (Ni) 14.0 – 16.0 0.15 under / over 13.85 – 16.15
Molybdenum (Mo) 1.00 – 1.40 0.05 under / over 0.95 – 1.45
Titanium (Ti) 0.30 – 0.60 0.05 under / over 0.25 – 0.65
Boron (B) 0.004 – 0.008 No A480 B row tabulated By agreement

Any row marked as a gap or by agreement in that table is a place where A480 does not tabulate a tolerance for the level this grade requires, and the acceptance band then has to be agreed in writing on the order. Product tolerances never apply to the heat analysis itself, which must stay inside Table 1.

Mechanical Properties of ASTM A312 UNS S31272

Table 4 sets the room-temperature tensile requirements that every lot of UNS S31272 pipe must meet after the final anneal. For this grade the minimums are 65 ksi [450 MPa] tensile and 29 ksi [200 MPa] yield, with elongation of 35% longitudinal / 25% transverse (general austenitic rule). The table below summarizes the row as it applies to this grade.

Property S31272
Tensile, min 65 ksi [450 MPa]
Yield, min 29 ksi [200 MPa]
Elongation 35% L / 25% T (general austenitic rule)

These are minimum values for acceptance, not design allowables. Allowable stresses for pressure design come from the governing piping code at the design temperature, and the code tables, not the A312 minimum, decide wall thickness. A312 does not assert a Table 4 hardness maximum for this grade, so if a hardness limit is needed for a specific service, write it on the purchase order.

At receiving, check that the tensile report quotes the right row for UNS S31272 rather than a generic 300-series line, that elongation is recorded with its direction, and that the specimen type matches the pipe size. Flattening tests and, where applicable, bend tests on welded pipe follow the A312 rules for the manufacturing type.

Dimensions, Tolerances and Stock Sizes

Dimensional supply for ASTM A312 UNS S31272 follows ASME B36.19 for standard NPS and schedule combinations, with special OD and wall by agreement when a project needs a section the schedules do not cover. Outside-diameter variations follow ASTM A999/A999M, and wall-thickness variations follow A312 Table 3, summarized below.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

Read the table by NPS band first, then by the wall-to-diameter ratio. The under-tolerance is 12.5% throughout, while the permitted over-tolerance varies with size and route. Whether the ordered wall is nominal or minimum (Supplementary S8) changes how those percentages are applied, so state it on the purchase order.

  • Lengths — single random, double random or cut-to-length as ordered
  • Ends — plain or bevelled; give bevel angle and root face when the WPS is already fixed
  • Jointers — not permitted unless the purchase order allows them

Stock / Available sizes. SHH STEEL quotes UNS S31272 against a practical stock-and-mill enquiry range rather than a frozen warehouse list. Because this is a UNS-only alloy, much of the volume is mill-order, and selected common sizes may be available from stock or remnant programmes. The table below shows the representative sizes we most often discuss; availability by route and wall must be confirmed on each enquiry, and we do not publish SKU numbers or tonnages.

Representative size Typical schedules / notes
NPS 1/2 – 2 Sch 40S / 80S; heater and instrument connections
NPS 3 – 8 Sch 10S / 40S / 80S; transfer and header lines
NPS 10 – 24 Sch 10S / 40S; often mill-order in either route
Special OD × wall By agreement; state OD, wall (nominal or minimum) and length practice

Typical examples we quote include 21.3 mm × 2.77 mm (NPS 1/2 Sch 40S), 60.3 mm × 3.91 mm (NPS 2 Sch 40S), 114.3 mm × 3.05 mm (NPS 4 Sch 10S) and 168.3 mm × 7.11 mm (NPS 6 Sch 40S). Special OD × wall, non-standard lengths and mixed SML/WLD packages are routine on enquiry; send the size list and we will separate what can ship from stock from what needs a mill slot.

Equivalent Grades

Equivalence for UNS S31272 is mainly an identity question. Under ASTM A312 the governing designation is the UNS number itself, and any trade name, European number or plate designation is only an engineering map back to the Table 1 row. The table below lists the references buyers most often bring to us, with how each relates to the A312 grade.

Designation How it relates to ASTM A312 UNS S31272
ASTM A312 / A312M UNS S31272 Governing pipe standard for this page; UNS identity only, no TP name
ASME SA-312 UNS S31272 Separate ASME Code standard; dual marking only when the purchase order names both
Proprietary maps Recheck Ti, B, Mo, C band

ASME SA-312 is listed because Code projects often need it, but it is a separate standard; when both marks are needed, the purchase order should name both and the mill certifies the heat against each. If a project specification quotes a brand name or EN number, ask for certification to ASTM A312 UNS S31272 and list any extra requirements separately rather than assuming the reference covers them.

Heat Treatment and Delivery Condition

All A312 pipe is furnished in the heat-treated condition. For UNS S31272 the solution anneal is 1920 °F [1050 °C] minimum, followed by quenching in water or rapid cooling by other means. Table 2 lists S31272 with S30815 at this temperature, slightly above the 1900 °F [1040 °C] default, so a habitual 316 anneal is not automatic compliance. The purpose is to put alloying elements back into solution and leave a clean, uniform austenitic structure before the pipe is tested and shipped.

UNS S31272 is not an H grade under A312, so the Table 5 grain-size requirement, clause 6.2 reheat rules and mandatory heat-treatment lot marking do not apply unless the owner specification adds them. The MTC should state the actual temperature and cooling method used, because a mill running mixed grades through one furnace may otherwise default to a neighbouring grade’s practice. If pipe is hot formed or heavily cold bent during fabrication, plan a full re-anneal to the same Table 2 practice where the governing code requires it, and confirm that the furnace can hold the temperature for the size before the work starts.

Corrosion Resistance

Corrosion is not the selection driver for S31272. With 14–16% chromium and 1.00–1.40% molybdenum it has less general and chloride corrosion margin than 316L, and its deliberately high carbon band means it should not be treated as a sensitization-proof grade in aqueous service just because titanium is present. Stabilization helps, but it is not a guarantee in a wet chloride environment.

Where S31272 earns its place is at temperature, where carbide stability and oxidation behaviour in the owner’s process matter more than pitting numbers. A312 contains no corrosion table for this grade, so any service claim should come from the owner’s materials engineer and, if needed, from project-specific testing.

Applications of ASTM A312 UNS S31272 Pipe

The source datasheet lists only owner-driven uses for this grade, which is honest: S31272 is ordered because a specification names it. They are starting points for selection, not approvals, and the owner’s materials engineer should confirm each against process data.

Application Why S31272 Note
Specialty high-temperature / process lines per project spec Ti+B + mid Mo Follow owner grade list
Engineered substitutions from proprietary specs UNS identity Verify every Table 1 limit

In every case the order should name ASTM A312 UNS S31272, the manufacturing route, size and wall, and the certificate requirements. Where a project also buys sister grades, keep them segregated through fabrication, because the Table 4 and Table 2 rows differ even when the pipes look identical on the rack.

Weldability

UNS S31272 pipe can be joined by GTAW, GMAW and SMAW when the procedure is qualified on the actual grade. On filler metal, Table 6 shows only an ellipsis for S31272, so no AWS filler class is assigned and the consumable must be agreed between purchaser and fabricator. Mill longitudinal welds on WLD and HCW pipe are autogenous, so the filler question applies only to fabrication welds made in the shop or on site.

Titanium- and boron-bearing weld metal can be sensitive to hot cracking, so heat input control and clean joint preparation matter. Because Table 6 shows no assigned filler, the consumable should reflect the elevated-temperature duty and be qualified on S31272 itself; do not assume ER316 or ER321 simply because the base metal contains Mo or Ti. Back-purge roots with argon, keep interpass temperature controlled, and remove heat tint by pickling or mechanical cleaning where the owner specification requires a clean surface.

Surface Finishes

Surface condition for ASTM A312 UNS S31272 pipe should be stated on the purchase order rather than left to the mill default. For stainless pipe, residual scale, embedded free iron and handling contamination can matter as much as the nominal finish name, particularly on corrosion-critical lines.

  • Annealed and pickled — the usual delivery condition after solution treatment
  • Blasted and pickled — when scale removal needs a mechanical assist before passivation
  • Bright annealed — by agreement for selected sizes and routes
  • Polished OD or ID — grit or Ra target by agreement; state which surface

Export orders should also state how ends are protected and that chloride-bearing labels or markers must not contact the bore. Those handling notes prevent avoidable rejections at receiving without changing the A312 metallurgical release.

Inspection and Testing

The base acceptance package for ASTM A312 UNS S31272 combines heat chemistry, tension testing against the Table 4 row, flattening or bend tests per the route, heat-treatment evidence and a hydrostatic or electric test on every length. Supplementary requirements are optional until they are written on the order; the table below lists the ones buyers request most often for this grade.

Option Purpose
S1 product analysis Confirms chemistry on finished pipe using A480 tolerances
S5 radiography Weld integrity on WLD pipe
S7 intergranular corrosion A262 Practice E check where the owner requires it
S8 minimum wall Wall interpreted as minimum rather than nominal
Project corrosion test For example ASTM G48, with method and acceptance agreed on the order

EN 10204 3.1 certification is our standard document set, and 3.2 third-party inspection is arranged when the enquiry names the agency and hold points. Hydrostatic versus electric testing should also be fixed on the purchase order if the project has a preference, because a silent mill option is not the same as an approved method.

Packaging and Shipping

Each length of UNS S31272 pipe is marked with ASTM A312, UNS S31272, manufacturing route, size, heat number and test method, with SA-312 added only when dual marking is ordered. Packing lists repeat the heat numbers so receiving can match pipe to certificates without opening every bundle.

  • End caps or bevel protectors as ordered
  • Bundles strapped with protected contact points to limit iron pick-up
  • Wooden cases or waterproof wrapping for ocean freight when specified
  • Packing list with heat numbers, sizes and certificate references

Tell us the destination and any handling limits early, so packing suits the transport route and the receiving site instead of being redone at the port, and so special marking such as project tag numbers can be applied at the mill.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless pipe and plate, and for ASTM A312 UNS S31272 we quote against the edition you name rather than a generic catalogue sheet. UNS-only grades are where generic sourcing goes wrong most often: a heat that looks close on paper can miss one Table 1 element, carry the wrong tensile row or skip the specified anneal. Our job is to catch those issues before the pipe is made, not after it arrives.

  • Full Table 1 chemistry for UNS S31272 on the MTC, including every range element
  • The correct Table 4 row (65/29 ksi) and the 1920 °F [1050 °C] minimum anneal stated on the certificate
  • Honest filler guidance based on what Table 6 does and does not say
  • SML, WLD and HCW routes with EN 10204 3.1 MTCs, and 3.2 inspection on request
  • Dual A312 / SA-312 marking only when the purchase order asks for both

If you are still choosing between UNS S31272 and its sister grades, send the service conditions, design temperature and preferred route; we will tell you plainly when a different A312 grade would fit better or cost less, rather than pushing whatever happens to be closest in name.

Supply Capability

SHH STEEL can supply ASTM A312 UNS S31272 pipe against the edition and route named on your enquiry. The capability table below summarizes the sizes, finishes and documents we regularly quote for this grade, and each line can be tightened on the purchase order.

Item SHH STEEL capability for UNS S31272
Standard ASTM A312 / A312M UNS S31272
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD and wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length Single random, double random or cut-to-length
Finish Annealed and pickled; blasted and pickled; bright annealed or polished by agreement
Heat treatment 1920 °F [1050 °C] minimum, rapid cool
Tensile 65/29 ksi
Documents EN 10204 3.1 with full Table 1 analysis; 3.2 on request
Trade terms FOB, CFR, CIF, EXW and other agreed Incoterms

Stock / Available sizes. The representative stock-and-mill range for UNS S31272 is shown in the Dimensions section (NPS 1/2–24 in typical Sch 10S/40S/80S combinations). Selected common sizes may ship from stock or remnant programmes, while heavy-wall seamless, unusual schedules and large quantities are normally mill-order; ask for a live check against your size list rather than relying on a catalogue claim.

A useful enquiry states the A312 edition, UNS S31272, route, NPS or OD × wall (nominal or minimum), quantity and length, finish, and any product analysis, corrosion test or 3.2 requirement. With that information we can confirm route, lead time and document package on the first reply instead of trading questions.

FAQ

Is ASTM A312 the same as ASME SA-312 for UNS S31272?
No. They are two independent standards: ASTM A312/A312M is the ASTM product specification, and ASME SA-312 is a separate Code standard used in Code piping. The UNS S31272 requirements usually run parallel, but if your project needs both, name both on the purchase order and ask for dual marking on a heat certified to each.
What chemistry defines ASTM A312 UNS S31272?
Table 1 sets C 0.08–0.12%, Mn 1.5–2.0%, Si 0.25–0.75%, Cr 14.0–16.0%, Ni 14.0–16.0%, Mo 1.00–1.40%, Ti 0.30–0.60% and B 0.004–0.008%. Every element with a range must be inside it on the heat analysis, and the MTC should report all of them as measured values. If S1 product analysis is ordered, A480 tolerances apply to the finished pipe only, never to the heat analysis.
UNS S31272 vs TP316Ti: are they interchangeable?
No. A312 TP316Ti is a 316-type grade with 16–18% Cr, 2–3% Mo and titanium stabilization for corrosion service. S31272 has 14–16% Cr, 14–16% Ni, a 0.08–0.12% carbon band, 1.00–1.40% Mo and boron, a 65/29 ksi floor and a 1920 °F anneal. Substituting either way changes the design basis.
What are the tensile requirements for ASTM A312 UNS S31272?
Table 4 requires 65 ksi [450 MPa] tensile and 29 ksi [200 MPa] yield, with elongation of 35% longitudinal / 25% transverse (general austenitic rule). These are acceptance minimums after the final anneal, not design allowables. Pressure design uses the governing code's allowable stress at temperature, which is why the code, not this table, sets the wall.
What heat treatment applies to ASTM A312 UNS S31272 pipe?
The pipe is solution annealed at 1920 °F [1050 °C] minimum and rapidly cooled. Table 2 lists S31272 with S30815 at this temperature, slightly above the 1900 °F [1040 °C] default, so a habitual 316 anneal is not automatic compliance. The certificate should state the actual temperature and cooling method. UNS S31272 is not an H grade, so there is no mandatory Table 5 grain-size test.
Why does S31272 contain boron?
Table 1 requires B 0.004–0.008% as a deliberate addition, which in creep-resistant austenitic steels is used to strengthen grain boundaries at temperature. A480 has no boron product-analysis tolerance row, so if S1 product analysis is ordered, the acceptance band for boron has to be agreed in writing with the supplier.
Is UNS S31272 an H grade under ASTM A312?
No. Although carbon is a 0.08–0.12% band, A312 does not class S31272 as an H grade, so the Table 5 grain-size requirement and clause 6.2 reheat rules for H grades are not mandatory. An owner specification may still add a grain-size check, and if it does, write it on the purchase order.
Seamless or welded UNS S31272 pipe: which should I order?
Seamless is usually chosen for small bores, heavy walls and owners who exclude welded pipe. Welded pipe, made without filler and then annealed, is often more economical in larger diameters and thin walls. Both must meet the same Table 1 chemistry and heat treatment; the design code and inspection plan decide.
What filler metal should be used to weld UNS S31272 pipe?
Table 6 shows only an ellipsis for S31272, so no AWS filler class is assigned and the consumable must be agreed between purchaser and fabricator. Whatever consumable is chosen, qualify it on UNS S31272 base metal, record the class on the WPS and PQR, and keep heat input and interpass temperature under control. The mill seam on WLD pipe is autogenous, so this applies only to fabrication welds.
Which sizes of ASTM A312 UNS S31272 pipe can SHH STEEL supply?
We quote NPS 1/8 upward to ASME B36.19 schedules such as 10S, 40S and 80S, plus special OD and wall by agreement. Representative enquiry sizes run from NPS 1/2 to 24; selected sizes may come from stock, and the rest are mill-order, confirmed size by size on each enquiry.
How should I check an MTC for ASTM A312 UNS S31272 pipe?
Confirm the certificate names ASTM A312/A312M and UNS S31272, reports every Table 1 element as a measured heat value, quotes the Table 4 row for this grade (65/29 ksi), and states the anneal temperature and cooling method. Then match heat numbers on the certificate to the pipe stencil and packing list.

Conclusion

ASTM A312 UNS S31272 is a titanium-boron stabilized 15Cr-15Ni-Mo grade with C 0.08–0.12%, Mn 1.5–2.0%, Si 0.25–0.75%, Cr 14.0–16.0%, Ni 14.0–16.0%, Mo 1.00–1.40%, Ti 0.30–0.60% and B 0.004–0.008%, a Table 4 floor of 65/29 ksi and a solution anneal at 1920 °F [1050 °C] minimum. It is ordered by UNS number, and it is not a drop-in replacement for A312 TP316Ti or any other sister grade. Put the A312 edition, route, size and wall, finish and any supplementary tests on the purchase order, then check the EN 10204 3.1 certificate against Table 1 and Table 4 before release. SHH STEEL can supply ASTM A312 UNS S31272 pipe to the edition you name; browse sister grades on the A312/A312M hub, or send your size list to admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X