ASTM A312 UNS S31002 Stainless Steel Pipe | ASTM A312 Stainless Steel - SHH STEEL

ASTM A312 UNS S31002 Stainless Steel Pipe

ASTM A312 UNS S31002 low-carbon low-silicon 25Cr-20Ni stainless steel pipe for nitric acid service, in SML, WLD and HCW, with C ≤0.015%, Si ≤0.15%, a 73/30 ksi Table 4 floor and a 1900 °F anneal, supplied by SHH STEEL with EN 10204 3.1 MTCs.
Grade
UNS S31002
Standard
ASTM A312 / A312M
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASTM A312 UNS S31002 Stainless Steel Pipe

A312/A312M is the ASTM product specification for seamless, welded, and heavily cold-worked austenitic stainless steel pipe intended for high-temperature and general corrosive service. It stands on its own as an ASTM standard, and this page is written against it. UNS S31002 is one of the less common rows in its Table 1, and that is exactly why buyers ask us to spell out what the specification actually fixes for this alloy and what is left to agreement between purchaser and mill.

UNS S31002 is the ultra-low-carbon, low-silicon version of the 25Cr-20Ni alloy, listed in A312 by UNS number only. It keeps the 24.0–26.0% chromium and 19.0–22.0% nickel of TP310S but limits carbon to 0.015%, silicon to 0.15%, molybdenum to 0.10%, and phosphorus and sulfur to 0.020% and 0.015%. Those tight limits make it a corrosion grade for nitric acid and other strongly oxidizing media rather than a furnace alloy, and its Table 4 floor is 73 ksi tensile and 30 ksi yield.

SHH STEEL can supply ASTM A312 UNS S31002 pipe as seamless (SML), welded (WLD), or heavily cold-worked (HCW) product, in ASME B36.19 stainless schedules or special OD and wall by agreement, with EN 10204 3.1 mill test certificates that report the full Table 1 heat analysis, the Table 4 tension results, and the heat-treatment record. Where a purchase order also asks for ASME SA-312 marking, dual marking can be offered on heats that qualify under both documents, but the ASTM grade remains the one this page describes.

Enquiries often call it 310L, low-carbon 310, or low-silicon 310, but those names cover several chemistries, so the order should read ASTM A312 UNS S31002. A heat that meets TP310S but not the 0.015% carbon and 0.15% silicon limits is not S31002, and the certificate needs to show both lines clearly.

If UNS S31002 turns out not to be the right fit, the closest sister pages in the same ASTM series are A312 TP310S, A312 UNS S31050, A312 TP310H, A312 UNS S30600, and A312 TP304L. All A312 grades are collected on the A312/A312M hub, so a short list can be compared against one standard before the enquiry goes out.

Manufacturing Types (SML / WLD / HCW)

ASTM A312 allows three manufacturing routes for UNS S31002 pipe, and the route is a purchase-order decision rather than a property of the grade. Whichever route is chosen, the heat must still meet the same Table 1 limits (C ≤0.015%, Mn ≤2.00%, P ≤0.020%, S ≤0.015%, Si ≤0.15%, Cr 24.0–26.0%, Ni 19.0–22.0%, Mo ≤0.10%, and N ≤0.10%), the same Table 4 tension floor, and the same 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling heat-treatment requirement before any length is released.

  • Seamless (SML) pierced and hot or cold finished, chosen for heavy wall, high pressure, or owner specifications that exclude a weld seam
  • Welded (WLD) formed from flat-rolled product and welded without filler or with filler where the edition allows, economical in thinner walls and larger diameters
  • Heavily cold-worked (HCW) welded pipe given at least 35% cold reduction of the weld and base metal before the final anneal, which refines the weld structure toward seamless behaviour

S31002 is a specialty corrosion alloy usually made seamless in small and medium sizes and welded in larger diameters, and it is frequently ordered by OD × wall for condensers and coolers rather than by NPS. Tell us which route your design code or client specification accepts, because a quotation that leaves the route open forces the mill to choose and can create disputes at receiving inspection.

Chemical Composition of ASTM A312 UNS S31002

The melting analysis in Table 1 is what the heat must meet when it is cast, and it is the first table a reviewer should compare against the mill certificate. For UNS S31002 the defining limits are C ≤0.015%, Mn ≤2.00%, P ≤0.020%, S ≤0.015%, Si ≤0.15%, Cr 24.0–26.0%, Ni 19.0–22.0%, Mo ≤0.10%, and N ≤0.10%. The table below reproduces the Table 1 row as published, with elements carrying no requirement shown as such rather than filled with invented values.

Element UNS S31002 melting analysis
Carbon (C) ≤ 0.015
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.020
Sulfur (S) ≤ 0.015
Silicon (Si) ≤ 0.15
Chromium (Cr) 24.0 – 26.0
Nickel (Ni) 19.0 – 22.0
Molybdenum (Mo) ≤ 0.10
Nitrogen (N) ≤ 0.10

Carbon at 0.015% maximum and silicon at 0.15% maximum are the two lines that define the grade; both are far below TP310S, and both matter in nitric acid, where silicon and carbides at grain boundaries promote intergranular attack. Chromium at 24–26% and nickel at 19–22% give the passive film its strength in oxidizing media.

Product analysis is a separate check made on the finished pipe, and ASTM A312 refers it to the permitted variations in ASTM A480 Table A1.1. The second table adds those tolerances to the melt limits so you can see the band that a check analysis on the pipe is allowed to fall within when Supplementary Requirement S1 or an owner check is ordered.

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) ≤ 0.015 0.005 over ≤ 0.020
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.020 0.005 over ≤ 0.025
Sulfur (S) ≤ 0.015 0.005 over ≤ 0.020
Silicon (Si) ≤ 0.15 0.05 over ≤ 0.20
Chromium (Cr) 24.0 – 26.0 0.25 under / over 23.75 – 26.25
Nickel (Ni) 19.0 – 22.0 0.15 under / 0.20 over 18.85 – 22.20
Molybdenum (Mo) ≤ 0.10 No A480 row below/at 0.20 start Not established—by agreement
Nitrogen (N) ≤ 0.10 0.01 over ≤ 0.11

Read the product limits as acceptance bounds for a check analysis only. A heat that sits outside the Table 1 melt range is non-conforming even if a later product analysis lands inside the widened band, so the certificate should always show the ladle analysis first. Molybdenum is capped at 0.10%, and A480 Table A1.1 gives no tolerance at that level, so a product-analysis allowance for Mo is by agreement.

Because S31002 is often confused with other 310 variants, the next table places its Table 1 row beside TP310S, TP310H, and TP310Cb.

Element TP310S TP310H TP310Cb UNS S31002
C ≤ 0.08 0.04 – 0.10 ≤ 0.08 ≤ 0.015
Si ≤ 1.00 ≤ 1.00 ≤ 1.00 ≤ 0.15
Mo ≤ 0.75 … ≤ 0.75 ≤ 0.10
Nb … … 10×C – 1.10 …
N … … … ≤ 0.10
H controls No Yes No No

Mechanical Properties of ASTM A312 UNS S31002

Table 4 sets the room-temperature tension requirements for UNS S31002: 73 ksi [500 MPa] tensile strength and 30 ksi [205 MPa] yield strength minimum, with elongation of 35% longitudinal / 25% transverse minimum. The table below shows those values in the form used on the specification, and the mill certificate should report actual results against each line.

Property UNS S31002
Tensile strength, min 73 ksi [500 MPa]
Yield strength, min 30 ksi [205 MPa]
Elongation, min 35% longitudinal / 25% transverse
Hardness No Table 4 maximum

The 73 ksi tensile floor is slightly lower than the 75 ksi of TP310S, reflecting the very low carbon, while the yield floor is the same 30 ksi. In nitric acid service the wall is normally set by corrosion allowance, and elevated-temperature allowables must come from the governing code for this UNS.

No hardness maximum is set for this grade in Table 4, so a hardness figure on a certificate is information rather than an acceptance criterion unless your order adds one. If a project specification imposes hardness or impact testing, write it on the purchase order so the mill can plan the test pieces before the pipe is cut.

Dimensions, Tolerances and Stock Sizes

Dimensions for ASTM A312 UNS S31002 pipe are normally ordered by NPS and schedule from ASME B36.19, or by outside diameter and wall where the design calls for a non-standard size. Outside-diameter tolerance and wall tolerance come from the specification itself, and wall is read as nominal unless Supplementary Requirement S8 asks for minimum wall. The permitted variations in wall thickness from Table 3 are shown below by NPS band and wall-to-diameter ratio.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

In practice the under-tolerance of 12.5% is the figure that matters for pressure design, because the designer has already sized the nominal wall with that allowance in mind. The over-tolerance varies with NPS and the wall-to-diameter ratio, which matters more for fit-up and weld preparation than for strength. For UNS S31002, whose higher strength or special chemistry often justifies a lighter or more closely engineered wall, confirm whether your calculation assumed nominal or minimum wall before the order is placed.

Stock / Available sizes. The table below shows the representative size band we quote for ASTM A312 UNS S31002, with example OD × wall combinations taken from B36.19 schedules. It is a supply and stock-enquiry range rather than a promise that every size sits on the floor today: for S31002 limited seamless sizes may be found as existing material, but most orders, especially OD × wall sizes for heat exchangers, are mill production. Special OD, special wall, and cut lengths are always handled on enquiry.

Representative size Example OD × wall Typical schedules / notes
NPS 1/2 – 2 21.34 × 2.77 mm (NPS 1/2 Sch 40S); 60.33 × 3.91 mm (NPS 2 Sch 40S) Sch 10S / 40S / 80S; small-bore process and instrument take-offs
NPS 2-1/2 – 6 88.90 × 5.49 mm (NPS 3 Sch 40S); 168.28 × 3.40 mm (NPS 6 Sch 10S) Sch 10S / 40S / 80S; the most frequent enquiry band
NPS 8 – 12 219.08 × 8.18 mm (NPS 8 Sch 40S); 323.85 × 4.57 mm (NPS 12 Sch 10S) Sch 10S / 40S; confirm SML or WLD route on enquiry
NPS 14 – 24 406.40 × 4.78 mm (NPS 16 Sch 10S); 609.60 × 9.53 mm (NPS 24 Sch 40S) Sch 10S / 40S; usually mill-order, mostly welded
Special OD × wall Any OD and wall the mill can qualify On enquiry: state OD, nominal or minimum wall, and length practice

Read the example sizes as orientation for writing the enquiry, not as a price list. When you send a size list we check live availability line by line, separate what can ship from existing material from what needs a mill slot, and give the lead time for each group so the purchase order can be split if the schedule demands it.

Equivalent Grades

Buyers often arrive with a trade name, a plate designation, or a European number rather than the A312 row. The table below maps the names we see on enquiries for UNS S31002, but only the ASTM A312 grade and UNS number are contractual on this page; everything else is a cross-reference that needs checking against its own standard.

Designation Notes
ASTM A312 UNS S31002 Governing grade on this page (no TP name)
ASME SA-312 UNS S31002 Separate Code standard; dual mark only when the order names both
310L / low-carbon 310 Trade names; confirm C ≤0.015 and Si ≤0.15
ASTM A240 S31002 Plate counterpart under a separate specification
EN / JIS No one-to-one equivalent asserted (EN 1.4335-type maps are engineering judgments)

The ASME SA-312 row is listed because some Code projects require it, not because it is a synonym. ASME SA-312 is a separate standard adopted into the Boiler and Pressure Vessel Code, and the SA312 UNS S31002 page covers that document on its own terms. When both marks are wanted, the order should name both specifications and their editions so the certificate can state compliance with each.

Heat Treatment and Delivery Condition

S31002 is not individually listed in Table 2, so it takes the default solution anneal at 1900 °F [1040 °C] minimum, followed by water quenching or another rapid cool fast enough to prevent carbide reprecipitation. The ultra-low carbon already limits sensitization, but a correct anneal and fast cool still matter because nitric acid is very sensitive to grain-boundary condition. Seamless pipe may be quenched directly after hot forming if it is not below the Table 2 minimum.

Delivery condition for UNS S31002 is solution annealed, then descaled by pickling or by blasting and pickling, straightened, and cut to the ordered length practice. HCW pipe receives its cold reduction before the final anneal, so cold work is never the delivered condition. Ask for the actual annealing temperature and cooling method to be recorded on the certificate, because a reviewer cannot otherwise confirm the Table 2 requirement from the document alone.

Corrosion Resistance

ASTM A312 contains no corrosion table, so the following is engineering commentary rather than a specification requirement. S31002 is designed for strongly oxidizing media, above all nitric acid, where very low carbon and silicon limit intergranular attack along grain boundaries. With 24–26% chromium it forms a robust passive film, and S7 testing to A262 Practice E is the usual way to document intergranular resistance on the order; specific acid-strength and temperature limits come from corrosion engineering, not from A312.

It has essentially no molybdenum, so it is not suited to chloride-bearing water or reducing acids, and it is not a carburization alloy despite its 310 base. Where hot-gas oxidation is the main concern, TP310S or TP310H is usually the better and cheaper choice.

Applications of ASTM A312 UNS S31002 Pipe

Applications for ASTM A312 UNS S31002 pipe are in nitric acid and oxidizing chemical service. The table below summarizes the typical uses we see.

Application Why S31002 Note
Nitric acid and oxidizing chemical lines Ultra-low C and Si Confirm concentration / temperature with corrosion engineering
High-temperature process with welded aqueous exposure Low sensitization risk Compare TP310S if Si ≤0.15% is not required
Furnace / hot gas with corrosion-critical shutdowns 310 oxidation + low C Not a carburization specialist
Condensers and coolers in oxidizing service Low C / low Si + 25Cr–20Ni Often ordered by OD × wall
Welded process piping needing as-welded IGC resistance C ≤0.015% limits HAZ sensitization Order S7 if proof is required

Treat the table as a starting point for discussion with the process licensor or corrosion engineer, not as an approval. Code allowable stresses, temperature limits, and any owner material lists decide whether UNS S31002 is acceptable on a given line, and those checks should be made before the pipe is ordered rather than after it arrives.

Weldability

S31002 welds with GTAW, GMAW, and SMAW using low heat input and clean practice, since keeping carbon and silicon pick-up low in the weld is what preserves its nitric acid resistance. Table 6 gives no AWS class for S31002, so filler selection is by agreement; low-carbon, low-silicon 310-type consumables are the usual choice, and the procedure should be qualified on S31002.

Qualify the procedure on UNS S31002 itself rather than on a convenient 304 coupon, because the qualification has to demonstrate the strength and soundness of this chemistry. Clean joint preparation, controlled heat input and interpass temperature, and a back-purged root are the normal baseline; the certificate for any WLD pipe should also state whether filler metal was used in the longitudinal seam.

Surface Finishes

Surface condition for ASTM A312 UNS S31002 pipe should be stated on the purchase order rather than left to mill default. On stainless pipe, residual scale, embedded free iron, and chloride contamination from handling can matter as much as the nominal finish name, and they are far easier to prevent at the mill than to correct on site.

  • Annealed and pickled the standard delivery after solution treatment for process piping
  • Blasted and pickled when heavier scale needs mechanical help before chemical descaling
  • Bright annealed by agreement, generally on smaller sizes where the furnace atmosphere can be controlled
  • Passivated or polished by agreement, with the method and acceptance criteria written on the order

For UNS S31002, a clean pickled finish with full removal of weld heat tint is important, since nitric acid service is sensitive to any surface condition that weakens the passive film. If the line will be inspected for surface iron, specify the test method at the enquiry stage so that the packing and handling plan supports it.

Inspection and Testing

The base acceptance package for ASTM A312 UNS S31002 pipe combines heat analysis, tension testing, the flattening or bend test that applies to the manufacturing type, and a hydrostatic or non-destructive electric test on every length. Visual and dimensional inspection confirm the size and surface before marking. For S31002 the carbon and silicon results deserve the closest review, followed by phosphorus, sulfur, and molybdenum; S7 intergranular testing is commonly added for nitric service.

Supplementary requirements are optional until they are written on the order. The options buyers request most often for this grade are summarized below, and each one adds test time that should be allowed for in the delivery schedule.

Option Purpose
S1 product analysis Confirms C, Si, Mo (by agreement), N, and other elements on finished pipe
S5 radiography Weld integrity on WLD pipe
S7 intergranular corrosion A262 Practice E after sensitizing treatment
S8 minimum wall Wall interpreted as minimum rather than nominal
S9 weld decay Compares weld and base-metal loss rates
OES / combustion Si and C verification; handheld XRF is limited for light elements

Third-party inspection, witness points, and EN 10204 3.2 certification are available when the order names the inspection agency. Agree the hold points before production starts, because witnessing a hydrotest or a tension test after the fact is not possible.

Packaging and Shipping

ASTM A312 UNS S31002 pipe is packed for handling and for ocean or land transport. Each length is marked with ASTM A312, the grade UNS S31002, the manufacturing type, size, heat number, and the test method used, with SA-312 added only when the order asks for dual marking. Bundle lists repeat the heat numbers so receiving can match pipe to certificates without opening every wrap.

  • End caps or bevel protectors fitted as ordered
  • Bundles strapped with protected contact points to limit iron pick-up
  • Wooden cases or seaworthy bundles for export, with moisture protection for sea freight
  • Small-bore or polished pipe cased separately where damage risk is higher

Stainless pipe should not be stored or lifted in contact with carbon steel, and for a specialty grade such as UNS S31002 it is worth keeping the material segregated by heat on arrival, since mixing it with common 304 stock is the most frequent cause of misuse on site.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless pipe, and for a specialty grade such as ASTM A312 UNS S31002 we quote against the edition you name rather than a generic catalogue sheet. We report the full Table 1 heat analysis, the Table 4 tension results, and the heat-treatment record, and we tell you early when a size or route is a mill order instead of letting the lead time surprise you.

  • Clear separation of S31002 from TP310S and other 310L-type names on the order and certificate
  • Clear advice on sister grades under ASTM A312, so UNS S31002 is not confused with a commoner alloy that looks similar on paper
  • Honest separation of specification requirements from producer or market guidance in every document we send
  • EN 10204 3.1 certificates as standard, with third-party inspection and 3.2 certification on request

The aim is a delivery that clears receiving inspection on the first review. That means the certificate, the stencil, and the purchase order all say the same thing about grade, UNS number, manufacturing type, size, and heat treatment, and that any agreed variation is written down before the pipe is made.

Supply Capability

SHH STEEL can supply ASTM A312 UNS S31002 stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade, and each line can be narrowed to your project specification.

Item SHH STEEL capability for UNS S31002
Standard ASTM A312 / A312M, UNS S31002
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD and wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length Single random, double random, or cut to length
Heat treatment 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling
Filler guidance No AWS class in Table 6; filler by agreement (low-C, low-Si 310-type)
Testing Tension (73/30 ksi), flattening or bend, hydrostatic or electric test per length; S1, S5, S7, S8, S9 on order
Documents EN 10204 3.1 with full Table 1 analysis; 3.2 and third-party inspection on request
Trade terms FOB, CFR, CIF, EXW and other agreed Incoterms

Stock / Available sizes. The representative band for UNS S31002 is NPS 1/2 to 24 in Sch 10S, 40S, and 80S as listed under Dimensions. Selected common OD × wall combinations may be available from existing material, while heavy-wall seamless, unusual schedules, and special cut lengths are normally mill orders. We do not publish stock part numbers or tonnage claims for this grade; ask for a live check against your size list instead.

Enquiries move fastest when they state the A312 edition, UNS S31002, the manufacturing type, NPS or OD × wall (and whether the wall is nominal or minimum), length practice, finish, and any product-analysis, corrosion-test, or 3.2 requirements. Dual SA-312 marking, bevelled ends, and cut lengths are available on confirmed orders when the order says so.

FAQ

Is ASTM A312 UNS S31002 the same as ASME SA-312 UNS S31002?
They are two independent standards. ASTM A312/A312M is the ASTM product specification, and ASME SA-312 is the separate document adopted into the Boiler and Pressure Vessel Code. The technical rows for UNS S31002 are closely aligned in current editions, but a pipe is only certified to the document named on the order, so when both are needed the purchase order should list both specifications and editions and the certificate should state compliance with each.
What is the UNS number for ASTM A312 UNS S31002?
This alloy has no TP name in A312 Table 1; it is ordered as UNS S31002, often described as 310L in the market. The UNS number should appear on the mill certificate and on the stencil next to the ASTM A312 mark, because a trade name alone makes it hard for receiving inspection to tie the chemistry on the certificate to the pipe in the rack.
What are the tensile and yield requirements for ASTM A312 UNS S31002 pipe?
Table 4 requires 73 ksi [500 MPa] tensile strength and 30 ksi [205 MPa] yield strength minimum, with elongation of 35% longitudinal / 25% transverse minimum. These are room-temperature minimums for acceptance only; design allowables at temperature come from the applicable piping code, and they should be checked there before a wall thickness is fixed.
What heat treatment does ASTM A312 UNS S31002 pipe receive?
S31002 is not individually listed in Table 2, so the default applies: solution anneal at 1900 °F [1040 °C] minimum, then water quench or rapid cool. The delivered condition is solution annealed and descaled, and the certificate should record the actual annealing temperature and the cooling method so a reviewer can confirm the requirement without asking the mill.
Which filler metal is used to weld ASTM A312 UNS S31002?
Table 6 gives no AWS A5.9 class for S31002, so filler selection is by agreement; low-carbon, low-silicon 310-type consumables are the usual choice to keep the weld’s nitric acid resistance. Whatever is chosen should be recorded on the WPS and PQR, and the procedure should be qualified on UNS S31002 base metal so that the joint strength and soundness are demonstrated on the real chemistry.
Is ASTM A312 UNS S31002 pipe available seamless and welded?
Yes. ASTM A312 allows seamless (SML), welded (WLD), and heavily cold-worked (HCW) pipe for UNS S31002, all meeting the same chemistry, tension, and heat-treatment rules. Seamless is usual for heavy wall and high pressure, while welded is often more economical in thin walls and larger diameters; state the accepted route on the order.
What sizes of ASTM A312 UNS S31002 pipe can SHH STEEL supply?
We quote NPS 1/2 to 24 in Sch 10S, 40S, and 80S as the representative band, plus NPS 1/8 and up and special OD and wall by agreement. Some common sizes may be available from existing material, while heavy-wall seamless and unusual schedules are normally mill orders, so send a size list for a live check.
What documents come with ASTM A312 UNS S31002 pipe?
Each shipment carries an EN 10204 3.1 mill test certificate showing the A312 edition, UNS S31002, manufacturing type, heat number, the full Table 1 heat analysis, Table 4 tension results, heat treatment, and the hydrostatic or electric test. Third-party inspection and 3.2 certification can be added when the order names the agency.
Is UNS S31002 the same as 310L?
310L is a market name that can cover several low-carbon 310 chemistries. UNS S31002 is the specific A312 row with carbon at 0.015% maximum, silicon at 0.15% maximum, and molybdenum at 0.10% maximum. Order by the UNS number so the certificate is checked against those exact limits.
Why is low silicon important in UNS S31002?
In hot nitric acid, silicon segregated to grain boundaries can accelerate intergranular attack, much as chromium carbides do. Holding silicon to 0.15% and carbon to 0.015% therefore gives S31002 better resistance than TP310S in this service, which is the main reason to choose it.
Can UNS S31002 be used in furnace service like TP310S?
It can tolerate high temperatures, but it is not optimized for them. Its very low carbon gives lower creep strength than TP310H, and its price reflects nitric acid duty. For hot-gas oxidation, TP310S or TP310H is normally the more appropriate choice.

Conclusion

ASTM A312 UNS S31002 (UNS S31002) is the ultra-low-carbon, low-silicon 25Cr-20Ni alloy of the series for nitric acid and oxidizing chemical service, with a 73/30 ksi floor and a 1900 °F default anneal. The specification fixes C ≤0.015%, Mn ≤2.00%, P ≤0.020%, S ≤0.015%, Si ≤0.15%, Cr 24.0–26.0%, Ni 19.0–22.0%, Mo ≤0.10%, and N ≤0.10%, a Table 4 floor of 73 ksi [500 MPa] tensile and 30 ksi [205 MPa] yield, and 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling heat treatment, while filler selection is by agreement because Table 6 gives no filler class for S31002. Put the manufacturing type, size and wall basis, finish, and any supplementary tests on the purchase order, and review the EN 10204 3.1 certificate against Tables 1, 2, and 4 before release. SHH STEEL can supply ASTM A312 UNS S31002 pipe to the edition you name; compare sister grades on the A312/A312M hub, or send your size list to admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X