ASTM A312 UNS S31050 Stainless Steel Pipe | ASTM A312 Stainless Steel - SHH STEEL

ASTM A312 UNS S31050 Stainless Steel Pipe

ASTM A312 UNS S31050 (310MoLN) stainless steel pipe for urea and carbamate service, in SML, WLD and HCW, with Cr 24–26%, Mo 1.60–2.60%, N 0.09–0.15%, an 84/39 ksi (t ≤0.250 in.) or 78/37 ksi Table 4 floor, supplied by SHH STEEL with EN 10204 3.1 MTCs.
Grade
UNS S31050
Standard
ASTM A312 / A312M
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASTM A312 UNS S31050 Stainless Steel Pipe

A312/A312M is the ASTM product specification for seamless, welded, and heavily cold-worked austenitic stainless steel pipe intended for high-temperature and general corrosive service. It stands on its own as an ASTM standard, and this page is written against it. UNS S31050 is one of the less common rows in its Table 1, and that is exactly why buyers ask us to spell out what the specification actually fixes for this alloy and what is left to agreement between purchaser and mill.

UNS S31050 is the 25Cr-22Ni-2Mo-N alloy of A312, listed by UNS number only and widely known as 310MoLN. It adds 1.60–2.60% molybdenum and 0.09–0.15% nitrogen to a low-carbon 310 base, with carbon at 0.025% and silicon at 0.40% maximum. The chemistry was developed for urea plants and other carbamate and oxidizing chemical service, and Table 4 gives it a wall-dependent tension floor rather than a single value.

SHH STEEL can supply ASTM A312 UNS S31050 pipe as seamless (SML), welded (WLD), or heavily cold-worked (HCW) product, in ASME B36.19 stainless schedules or special OD and wall by agreement, with EN 10204 3.1 mill test certificates that report the full Table 1 heat analysis, the Table 4 tension results, and the heat-treatment record. Where a purchase order also asks for ASME SA-312 marking, dual marking can be offered on heats that qualify under both documents, but the ASTM grade remains the one this page describes.

Order it as ASTM A312 UNS S31050; 310MoLN and European references such as EN 1.4466 are cross-references only and must be checked line by line. Urea licensors often add their own requirements beyond Table 1, so the licensor’s grade list should be attached to the enquiry.

If UNS S31050 turns out not to be the right fit, the closest sister pages in the same ASTM series are A312 UNS S31002, A312 TP310S, A312 UNS S31254, A312 TP316L, and A312 TP317L. All A312 grades are collected on the A312/A312M hub, so a short list can be compared against one standard before the enquiry goes out.

Manufacturing Types (SML / WLD / HCW)

ASTM A312 allows three manufacturing routes for UNS S31050 pipe, and the route is a purchase-order decision rather than a property of the grade. Whichever route is chosen, the heat must still meet the same Table 1 limits (C ≤0.025%, Mn ≤2.00%, P ≤0.020%, S ≤0.015%, Si ≤0.40%, Cr 24.0–26.0%, Ni 20.5–23.5%, Mo 1.60–2.60%, and N 0.09–0.15%), the same Table 4 tension floor, and the same 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling heat-treatment requirement before any length is released.

  • Seamless (SML) pierced and hot or cold finished, chosen for heavy wall, high pressure, or owner specifications that exclude a weld seam
  • Welded (WLD) formed from flat-rolled product and welded without filler or with filler where the edition allows, economical in thinner walls and larger diameters
  • Heavily cold-worked (HCW) welded pipe given at least 35% cold reduction of the weld and base metal before the final anneal, which refines the weld structure toward seamless behaviour

S31050 for urea service is most often seamless, particularly in high-pressure loops, and the wall thickness should be confirmed early because it decides which Table 4 row applies. Tell us which route your design code or client specification accepts, because a quotation that leaves the route open forces the mill to choose and can create disputes at receiving inspection.

Chemical Composition of ASTM A312 UNS S31050

The melting analysis in Table 1 is what the heat must meet when it is cast, and it is the first table a reviewer should compare against the mill certificate. For UNS S31050 the defining limits are C ≤0.025%, Mn ≤2.00%, P ≤0.020%, S ≤0.015%, Si ≤0.40%, Cr 24.0–26.0%, Ni 20.5–23.5%, Mo 1.60–2.60%, and N 0.09–0.15%. The table below reproduces the Table 1 row as published, with elements carrying no requirement shown as such rather than filled with invented values.

Element UNS S31050 melting analysis
Carbon (C) ≤ 0.025
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.020
Sulfur (S) ≤ 0.015
Silicon (Si) ≤ 0.40
Chromium (Cr) 24.0 – 26.0
Nickel (Ni) 20.5 – 23.5
Molybdenum (Mo) 1.60 – 2.60
Nitrogen (N) 0.09 – 0.15

Molybdenum at 1.60–2.60% and nitrogen at 0.09–0.15% are the defining additions, and together with 24–26% chromium they give the alloy its resistance to carbamate. Carbon at 0.025% and silicon at 0.40% maximum are held low to protect welds and grain boundaries, and nickel at 20.5–23.5% is a little higher than TP310S.

Product analysis is a separate check made on the finished pipe, and ASTM A312 refers it to the permitted variations in ASTM A480 Table A1.1. The second table adds those tolerances to the melt limits so you can see the band that a check analysis on the pipe is allowed to fall within when Supplementary Requirement S1 or an owner check is ordered.

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) ≤ 0.025 0.005 over ≤ 0.030
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.020 0.005 over ≤ 0.025
Sulfur (S) ≤ 0.015 0.005 over ≤ 0.020
Silicon (Si) ≤ 0.40 0.05 over ≤ 0.45
Chromium (Cr) 24.0 – 26.0 0.25 under / over 23.75 – 26.25
Nickel (Ni) 20.5 – 23.5 0.20 under / over 20.30 – 23.70
Molybdenum (Mo) 1.60 – 2.60 0.05 under / over 1.55 – 2.65
Nitrogen (N) 0.09 – 0.15 0.01 under / over 0.08 – 0.16

Read the product limits as acceptance bounds for a check analysis only. A heat that sits outside the Table 1 melt range is non-conforming even if a later product analysis lands inside the widened band, so the certificate should always show the ladle analysis first.

The next table compares S31050 with TP310S, S31002, and the 6Mo alloy S31254, which helps place each in its proper service niche.

Element TP310S UNS S31002 UNS S31050 UNS S31254
C ≤ 0.08 ≤ 0.015 ≤ 0.025 ≤ 0.020
Si ≤ 1.00 ≤ 0.15 ≤ 0.40 ≤ 0.80
Ni 19.0 – 22.0 19.0 – 22.0 20.5 – 23.5 17.5 – 18.5
Mo ≤ 0.75 ≤ 0.10 1.60 – 2.60 6.0 – 6.5
N … ≤ 0.10 0.09 – 0.15 0.18 – 0.22
Primary niche Hot oxidation Nitric / low C-Si Urea / carbamate Seawater / 6Mo

Mechanical Properties of ASTM A312 UNS S31050

Table 4 sets the room-temperature tension requirements for UNS S31050: 84 ksi [580 MPa] for walls up to 0.250 in. [6.35 mm] and 78 ksi [540 MPa] for heavier walls tensile strength and 39 ksi [270 MPa] and 37 ksi [255 MPa] respectively yield strength minimum, with elongation of 25% longitudinal minimum (transverse not separately stated). The table below shows those values in the form used on the specification, and the mill certificate should report actual results against each line.

Wall thickness t Tensile min Yield min
t ≤ 0.250 in. [6.35 mm] 84 ksi [580 MPa] 39 ksi [270 MPa]
t > 0.250 in. [6.35 mm] 78 ksi [540 MPa] 37 ksi [255 MPa]

Table 4 splits S31050 by wall: up to 0.250 in. [6.35 mm] the floor is 84 ksi tensile and 39 ksi yield, and above that it drops to 78 ksi and 37 ksi. Elongation is 25% longitudinal, the value grouped with S32615 in Table 4, and a transverse value is not stated separately, so confirm which wall row applies before reviewing the certificate.

No hardness maximum is set for this grade in Table 4, so a hardness figure on a certificate is information rather than an acceptance criterion unless your order adds one. If a project specification imposes hardness or impact testing, write it on the purchase order so the mill can plan the test pieces before the pipe is cut.

Dimensions, Tolerances and Stock Sizes

Dimensions for ASTM A312 UNS S31050 pipe are normally ordered by NPS and schedule from ASME B36.19, or by outside diameter and wall where the design calls for a non-standard size. Outside-diameter tolerance and wall tolerance come from the specification itself, and wall is read as nominal unless Supplementary Requirement S8 asks for minimum wall. The permitted variations in wall thickness from Table 3 are shown below by NPS band and wall-to-diameter ratio.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

In practice the under-tolerance of 12.5% is the figure that matters for pressure design, because the designer has already sized the nominal wall with that allowance in mind. The over-tolerance varies with NPS and the wall-to-diameter ratio, which matters more for fit-up and weld preparation than for strength. For UNS S31050, whose higher strength or special chemistry often justifies a lighter or more closely engineered wall, confirm whether your calculation assumed nominal or minimum wall before the order is placed.

Stock / Available sizes. The table below shows the representative size band we quote for ASTM A312 UNS S31050, with example OD × wall combinations taken from B36.19 schedules. It is a supply and stock-enquiry range rather than a promise that every size sits on the floor today: for S31050 most sizes, and nearly all urea high-pressure pipe, are planned as mill orders against the licensor’s requirements. Special OD, special wall, and cut lengths are always handled on enquiry.

Representative size Example OD × wall Typical schedules / notes
NPS 1/2 – 2 21.34 × 2.77 mm (NPS 1/2 Sch 40S); 60.33 × 3.91 mm (NPS 2 Sch 40S) Sch 10S / 40S / 80S; small-bore process and instrument take-offs
NPS 2-1/2 – 6 88.90 × 5.49 mm (NPS 3 Sch 40S); 168.28 × 3.40 mm (NPS 6 Sch 10S) Sch 10S / 40S / 80S; the most frequent enquiry band
NPS 8 – 12 219.08 × 8.18 mm (NPS 8 Sch 40S); 323.85 × 4.57 mm (NPS 12 Sch 10S) Sch 10S / 40S; confirm SML or WLD route on enquiry
NPS 14 – 24 406.40 × 4.78 mm (NPS 16 Sch 10S); 609.60 × 9.53 mm (NPS 24 Sch 40S) Sch 10S / 40S; usually mill-order, mostly welded
Special OD × wall Any OD and wall the mill can qualify On enquiry: state OD, nominal or minimum wall, and length practice

Read the example sizes as orientation for writing the enquiry, not as a price list. When you send a size list we check live availability line by line, separate what can ship from existing material from what needs a mill slot, and give the lead time for each group so the purchase order can be split if the schedule demands it.

Equivalent Grades

Buyers often arrive with a trade name, a plate designation, or a European number rather than the A312 row. The table below maps the names we see on enquiries for UNS S31050, but only the ASTM A312 grade and UNS number are contractual on this page; everything else is a cross-reference that needs checking against its own standard.

Designation Notes
ASTM A312 UNS S31050 Governing grade on this page (no TP name)
ASME SA-312 UNS S31050 Separate Code standard; dual mark only when the order names both
310MoLN (trade) Confirm the full Table 1 row incl. Si, Mo, and N
EN 1.4466 / X1CrNiMoN25-22-2 approx. Engineering map; recheck every limit before dual certification
ASTM A240 S31050 Plate counterpart under a separate specification

The ASME SA-312 row is listed because some Code projects require it, not because it is a synonym. ASME SA-312 is a separate standard adopted into the Boiler and Pressure Vessel Code, and the SA312 UNS S31050 page covers that document on its own terms. When both marks are wanted, the order should name both specifications and their editions so the certificate can state compliance with each.

Heat Treatment and Delivery Condition

S31050 is not individually listed in Table 2, so it takes the default solution anneal at 1900 °F [1040 °C] minimum, followed by water quenching or another rapid cool sufficient to prevent carbide reprecipitation. Urea licensors frequently add their own heat-treatment, ferrite, and corrosion-test requirements, and those must be written on the order. Seamless pipe may be quenched directly after hot forming if it is not below the Table 2 minimum.

Delivery condition for UNS S31050 is solution annealed, then descaled by pickling or by blasting and pickling, straightened, and cut to the ordered length practice. HCW pipe receives its cold reduction before the final anneal, so cold work is never the delivered condition. Ask for the actual annealing temperature and cooling method to be recorded on the certificate, because a reviewer cannot otherwise confirm the Table 2 requirement from the document alone.

Corrosion Resistance

ASTM A312 contains no corrosion table, so the following is engineering commentary rather than a specification requirement. S31050 was developed for urea synthesis, where ammonium carbamate is highly corrosive to ordinary stainless steels. Molybdenum and nitrogen on a 25Cr-22Ni base give it a stable passive film in that service, and low carbon and silicon protect welds and grain boundaries. Licensors usually require Huey-type corrosion testing and microstructural checks beyond A312, so their specification governs acceptance.

Outside urea plants it performs well in other oxidizing chemical service, and S7 intergranular testing can be ordered where proof is needed. It is not a seawater alloy, and for chloride-bearing water a 6Mo grade such as UNS S31254 is the more appropriate comparison.

Applications of ASTM A312 UNS S31050 Pipe

Applications for ASTM A312 UNS S31050 pipe are concentrated in urea plants and related chemical service. The table below summarizes the typical uses.

Application Why S31050 Note
Urea plant high-pressure piping 310MoLN chemistry (Mo + N) Follow licensor grade list
Urea strippers / condensers Low C/Si + intentional Mo/N Often seamless; confirm wall for Table 4 row
Oxidizing chemical lines Low C/Si + Mo/N Confirm concentration / temperature
Carbamate service Designed urea-grade alloy Not a seawater 6Mo substitute
Welded process piping needing as-welded IGC resistance C ≤0.025% limits HAZ sensitization Order S7 if proof is required

Treat the table as a starting point for discussion with the process licensor or corrosion engineer, not as an approval. Code allowable stresses, temperature limits, and any owner material lists decide whether UNS S31050 is acceptable on a given line, and those checks should be made before the pipe is ordered rather than after it arrives.

Weldability

S31050 welds with GTAW, GMAW, and SMAW using low heat input and careful cleanliness, since urea service is sensitive to weld-metal ferrite and contamination. Table 6 assigns no AWS class to S31050, so filler choice is by agreement, usually a matching 25-22-2 consumable specified by the licensor. Qualify the procedure on S31050 and include any licensor ferrite or corrosion-test requirements in the PQR.

Qualify the procedure on UNS S31050 itself rather than on a convenient 304 coupon, because the qualification has to demonstrate the strength and soundness of this chemistry. Clean joint preparation, controlled heat input and interpass temperature, and a back-purged root are the normal baseline; the certificate for any WLD pipe should also state whether filler metal was used in the longitudinal seam.

Surface Finishes

Surface condition for ASTM A312 UNS S31050 pipe should be stated on the purchase order rather than left to mill default. On stainless pipe, residual scale, embedded free iron, and chloride contamination from handling can matter as much as the nominal finish name, and they are far easier to prevent at the mill than to correct on site.

  • Annealed and pickled the standard delivery after solution treatment for process piping
  • Blasted and pickled when heavier scale needs mechanical help before chemical descaling
  • Bright annealed by agreement, generally on smaller sizes where the furnace atmosphere can be controlled
  • Passivated or polished by agreement, with the method and acceptance criteria written on the order

For UNS S31050, urea plant piping is normally supplied pickled with full removal of heat tint and iron contamination, and the licensor may add surface requirements. If the line will be inspected for surface iron, specify the test method at the enquiry stage so that the packing and handling plan supports it.

Inspection and Testing

The base acceptance package for ASTM A312 UNS S31050 pipe combines heat analysis, tension testing, the flattening or bend test that applies to the manufacturing type, and a hydrostatic or non-destructive electric test on every length. Visual and dimensional inspection confirm the size and surface before marking. For S31050 check molybdenum, nitrogen, carbon, and silicon first, confirm which wall-dependent Table 4 row applies, and plan for any licensor corrosion or microstructural tests in the schedule.

Supplementary requirements are optional until they are written on the order. The options buyers request most often for this grade are summarized below, and each one adds test time that should be allowed for in the delivery schedule.

Option Purpose
S1 product analysis Confirms C, Si, Mo, N, and other elements on finished pipe
S5 radiography Weld integrity on WLD pipe
S7 intergranular corrosion A262 Practice E after sensitizing treatment
S8 minimum wall Wall interpreted as minimum rather than nominal (also affects Table 4 row)
S9 weld decay Compares weld and base-metal loss rates
Licensor extras Huey / corrosion coupons when urea licensor specs require them

Third-party inspection, witness points, and EN 10204 3.2 certification are available when the order names the inspection agency. Agree the hold points before production starts, because witnessing a hydrotest or a tension test after the fact is not possible.

Packaging and Shipping

ASTM A312 UNS S31050 pipe is packed for handling and for ocean or land transport. Each length is marked with ASTM A312, the grade UNS S31050, the manufacturing type, size, heat number, and the test method used, with SA-312 added only when the order asks for dual marking. Bundle lists repeat the heat numbers so receiving can match pipe to certificates without opening every wrap.

  • End caps or bevel protectors fitted as ordered
  • Bundles strapped with protected contact points to limit iron pick-up
  • Wooden cases or seaworthy bundles for export, with moisture protection for sea freight
  • Small-bore or polished pipe cased separately where damage risk is higher

Stainless pipe should not be stored or lifted in contact with carbon steel, and for a specialty grade such as UNS S31050 it is worth keeping the material segregated by heat on arrival, since mixing it with common 304 stock is the most frequent cause of misuse on site.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless pipe, and for a specialty grade such as ASTM A312 UNS S31050 we quote against the edition you name rather than a generic catalogue sheet. We report the full Table 1 heat analysis, the Table 4 tension results, and the heat-treatment record, and we tell you early when a size or route is a mill order instead of letting the lead time surprise you.

  • Familiarity with urea-grade S31050 orders, including wall-dependent Table 4 rows and licensor add-on requirements
  • Clear advice on sister grades under ASTM A312, so UNS S31050 is not confused with a commoner alloy that looks similar on paper
  • Honest separation of specification requirements from producer or market guidance in every document we send
  • EN 10204 3.1 certificates as standard, with third-party inspection and 3.2 certification on request

The aim is a delivery that clears receiving inspection on the first review. That means the certificate, the stencil, and the purchase order all say the same thing about grade, UNS number, manufacturing type, size, and heat treatment, and that any agreed variation is written down before the pipe is made.

Supply Capability

SHH STEEL can supply ASTM A312 UNS S31050 stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade, and each line can be narrowed to your project specification.

Item SHH STEEL capability for UNS S31050
Standard ASTM A312 / A312M, UNS S31050
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD and wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length Single random, double random, or cut to length
Heat treatment 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling
Filler guidance No AWS class in Table 6; filler by agreement (matching 25-22-2 type)
Testing Tension (84/39 or 78/37 ksi by wall), flattening or bend, hydrostatic or electric test per length; S1, S5, S7, S8, S9 on order
Documents EN 10204 3.1 with full Table 1 analysis; 3.2 and third-party inspection on request
Trade terms FOB, CFR, CIF, EXW and other agreed Incoterms

Stock / Available sizes. The representative band for UNS S31050 is NPS 1/2 to 24 in Sch 10S, 40S, and 80S as listed under Dimensions. Selected common OD × wall combinations may be available from existing material, while heavy-wall seamless, unusual schedules, and special cut lengths are normally mill orders. We do not publish stock part numbers or tonnage claims for this grade; ask for a live check against your size list instead.

Enquiries move fastest when they state the A312 edition, UNS S31050, the manufacturing type, NPS or OD × wall (and whether the wall is nominal or minimum), length practice, finish, and any product-analysis, corrosion-test, or 3.2 requirements. Dual SA-312 marking, bevelled ends, and cut lengths are available on confirmed orders when the order says so.

FAQ

Is ASTM A312 UNS S31050 the same as ASME SA-312 UNS S31050?
They are two independent standards. ASTM A312/A312M is the ASTM product specification, and ASME SA-312 is the separate document adopted into the Boiler and Pressure Vessel Code. The technical rows for UNS S31050 are closely aligned in current editions, but a pipe is only certified to the document named on the order, so when both are needed the purchase order should list both specifications and editions and the certificate should state compliance with each.
What is the UNS number for ASTM A312 UNS S31050?
This alloy has no TP name in A312 Table 1; it is ordered as UNS S31050 and is widely known as 310MoLN. The UNS number should appear on the mill certificate and on the stencil next to the ASTM A312 mark, because a trade name alone makes it hard for receiving inspection to tie the chemistry on the certificate to the pipe in the rack.
What are the tensile and yield requirements for ASTM A312 UNS S31050 pipe?
Table 4 requires 84 ksi [580 MPa] for walls up to 0.250 in. [6.35 mm] and 78 ksi [540 MPa] for heavier walls tensile strength and 39 ksi [270 MPa] and 37 ksi [255 MPa] respectively yield strength minimum, with elongation of 25% longitudinal minimum (transverse not separately stated). These are room-temperature minimums for acceptance only; design allowables at temperature come from the applicable piping code, and they should be checked there before a wall thickness is fixed.
What heat treatment does ASTM A312 UNS S31050 pipe receive?
S31050 is not individually listed in Table 2, so the default applies: solution anneal at 1900 °F [1040 °C] minimum and water quench or rapid cool; urea licensors may add requirements. The delivered condition is solution annealed and descaled, and the certificate should record the actual annealing temperature and the cooling method so a reviewer can confirm the requirement without asking the mill.
Which filler metal is used to weld ASTM A312 UNS S31050?
Table 6 gives no AWS A5.9 class for S31050, so filler choice is by agreement, normally a matching 25-22-2 consumable named by the urea licensor and recorded on the WPS and PQR. Whatever is chosen should be recorded on the WPS and PQR, and the procedure should be qualified on UNS S31050 base metal so that the joint strength and soundness are demonstrated on the real chemistry.
Is ASTM A312 UNS S31050 pipe available seamless and welded?
Yes. ASTM A312 allows seamless (SML), welded (WLD), and heavily cold-worked (HCW) pipe for UNS S31050, all meeting the same chemistry, tension, and heat-treatment rules. Seamless is usual for heavy wall and high pressure, while welded is often more economical in thin walls and larger diameters; state the accepted route on the order.
What sizes of ASTM A312 UNS S31050 pipe can SHH STEEL supply?
We quote NPS 1/2 to 24 in Sch 10S, 40S, and 80S as the representative band, plus NPS 1/8 and up and special OD and wall by agreement. Some common sizes may be available from existing material, while heavy-wall seamless and unusual schedules are normally mill orders, so send a size list for a live check.
What documents come with ASTM A312 UNS S31050 pipe?
Each shipment carries an EN 10204 3.1 mill test certificate showing the A312 edition, UNS S31050, manufacturing type, heat number, the full Table 1 heat analysis, Table 4 tension results, heat treatment, and the hydrostatic or electric test. Third-party inspection and 3.2 certification can be added when the order names the agency.
Why does UNS S31050 have two strength levels in Table 4?
Table 4 sets 84 ksi tensile and 39 ksi yield for walls up to 0.250 in. [6.35 mm], and 78 ksi and 37 ksi for heavier walls. The specification simply sets a lower floor for the heavier wall range, so the certificate should be reviewed against the row that matches the ordered wall.
Is UNS S31050 the same as 310MoLN?
310MoLN is the common market name for this chemistry, but A312 orders it by UNS number. The contractual limits are those in Table 1, including Si ≤0.40%, Mo 1.60–2.60%, and N 0.09–0.15%, and urea licensors often add their own tighter requirements on top.
Can UNS S31050 replace a 6Mo alloy in seawater?
No. S31050 is designed for urea and carbamate service, and its 1.60–2.60% molybdenum is far below the 6.0–6.5% of UNS S31254. For seawater and chloride-bearing water, a 6Mo super-austenitic or a suitable duplex grade is the correct comparison.

Conclusion

ASTM A312 UNS S31050 (UNS S31050) is the 310MoLN urea-grade alloy of the series, with Mo 1.60–2.60% and N 0.09–0.15% on a low-carbon 25Cr-22Ni base and a wall-dependent Table 4 floor. The specification fixes C ≤0.025%, Mn ≤2.00%, P ≤0.020%, S ≤0.015%, Si ≤0.40%, Cr 24.0–26.0%, Ni 20.5–23.5%, Mo 1.60–2.60%, and N 0.09–0.15%, a Table 4 floor of 84 ksi [580 MPa] for walls up to 0.250 in. [6.35 mm] and 78 ksi [540 MPa] for heavier walls tensile and 39 ksi [270 MPa] and 37 ksi [255 MPa] respectively yield, and 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling heat treatment, while filler selection is by agreement because Table 6 gives no AWS class for S31050. Put the manufacturing type, size and wall basis, finish, and any supplementary tests on the purchase order, and review the EN 10204 3.1 certificate against Tables 1, 2, and 4 before release. SHH STEEL can supply ASTM A312 UNS S31050 pipe to the edition you name; compare sister grades on the A312/A312M hub, or send your size list to admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X