ASTM A213 TP347HFG Stainless Steel Tube | ASTM A213 Stainless Steel - SHH STEEL

ASTM A213 TP347HFG Stainless Steel Tube

ASTM A213 TP347HFG / UNS S34710 seamless boiler, superheater and heat-exchanger tube with carbon 0.06–0.10%, Cr 17.0–19.0%, Ni 9.0–13.0%, niobium ≥8×C ≤1.10%, Table 4 floor 80/30 ksi, hardness max 192 HBW / 90 HRB, ASTM grain size No. 7 to 10, and cold-finished manufacture only after Footnote I softening. SHH STEEL supplies cold-finished seamless tube with EN 10204 3.1 MTCs that report Nb, grain size, and the 2150 °F solution path.
Grade
TP347HFG / UNS S34710
Standard
ASTM A213 / A213M
Product form
Seamless boiler / superheater / heat-exchanger tube (cold-finished only — A213 6.1)
Size
Typical OD × min wall (or average wall) within ~1/8 in. [3.2 mm] ID to 5 in. [127 mm] OD and ~0.015–0.500 in. [0.4–12.7 mm] wall; other diameters by agreement
Share:
Overview
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASTM A213 TP347HFG Stainless Steel Tube

ASTM A213 / A213M is the ASTM International product specification for seamless ferritic and austenitic alloy-steel boiler, superheater, and heat-exchanger tubes. Grade TP347HFG / UNS S34710 is the fine-grain, niobium-stabilized high-temperature member of the 347 family — the letters “HFG” signal fine grain, not a casual shop nickname for ordinary 347H. Melting carbon sits in a tighter 0.06–0.10% band (a higher floor than TP347H’s 0.04%), chromium 17.0–19.0%, nickel 9.0–13.0%, and niobium is held at ≥8 × C and ≤1.10%. The heat-treatment path requires ASTM grain size No. 7 to 10 (a band with both coarse and fine bounds), solution treatment at 2150 °F [1175 °C] with Footnote I softening before cold working, and — uniquely among the common 347 rows — cold-finished manufacture only under A213 clause 6.1. That package exists for creep-range boiler and superheater service where fine-grain control and the higher Table 4 tensile floor share one datasheet — not as a synonym stamp for A213 TP347H.

SHH STEEL can supply ASTM A213 TP347HFG stainless steel tube as seamless cold-finished product in the usual boiler and heat-exchanger OD × wall / BWG band, shipped with EN 10204 3.1 mill test certificates that report the full ladle chemistry (including niobium against the 8 × C formula), the Table 4 tensile and hardness results (80 ksi tensile floor), and the grain-size result inside the 7–10 band for the heat-treatment lot. When a project also needs ASME Code Book marking, we dual-mark A213 / SA-213 on the same lengths only if the purchase order says so. Browse the grade family on the A213/A213M hub.

Commercially, TP347HFG tube is still called 347HFG, S34710, or fine-grain 347H boiler tube; none of those shop names replace the ASTM grade on the MTC or stencil. Sister grades under the same ASTM standard include A213 TP347H, A213 TP347, A213 TP321H, and A213 TP304H. A213 covers seamless tube only — no welded or HCW manufacturing type — and for TP347HFG the process choice is further restricted: cold-finished seamless only, not hot-finished. Do not order “347H hot-finished” and expect HFG acceptance.

Chemical Composition of A213 TP347HFG

Two chemistry layers matter for TP347HFG under ASTM A213. Melting (heat or ladle) analysis is mandatory for every heat; product analysis on finished tube applies only when Supplementary Requirement wording or the purchase order invokes it through ASTM A1016/A1016M. Product-analysis tolerances typically flow from ASTM A480/A480M Table A1.1. SHH STEEL reports actual ladle values — and product values when ordered — and does not advertise unpublished tighter catalogue windows. Three chemistry lines define the grade for a reviewer beside the process rules: carbon 0.06–0.10% (higher floor than TP347H), niobium ≥8 × C ≤1.10% (same formula as TP347H, not the non-H 10 × C rule), and chromium/nickel 17.0–19.0% / 9.0–13.0%. The fine-grain and cold-finished rules live in manufacture and heat-treatment clauses, not in a unique Nb formula.

The tables below reproduce the heat analysis for TP347HFG / UNS S34710, the product-analysis limits from A480 Table A1.1 practice, and a short carbon / grain / tensile snapshot against TP347H and TP347. Later A213 editions place austenitic stainless grades in Table 2 (older editions used Table 1); confirm the ordered edition on the purchase order. Creep-rupture allowables that buyers associate with “fine-grain 347H” are design-code language — A213 itself publishes the chemistry, grain band, and tensile floors, not a creep curve on the product page.

Melting analysis (heat / ladle analysis)

Element TP347HFG (UNS S34710) melting analysis
Carbon (C) 0.06 – 0.10
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.030
Silicon (Si) ≤ 1.00
Chromium (Cr) 17.0 – 19.0
Nickel (Ni) 9.0 – 13.0
Molybdenum (Mo) … (no requirement)
Nitrogen (N) … (no requirement)
Niobium (Nb / Cb) ≥ 8 × C, ≤ 1.10
Titanium (Ti) … (no requirement)

Source: ASTM A213/A213M stainless chemistry table for Grade TP347HFG / UNS S34710 (public mill / specification PDF excerpt — _ref_a213.txt / A213–13 table text). Confirm the ordered edition. Where ellipses appear, the ordered edition sets no requirement for that element. UNCERTAIN: exact edition year on the purchase order; stainless chemistry table number (Table 2 later / Table 1 older).

Product analysis — A480/A480M Table A1.1 tolerances applied

Element Melting Tolerance (A480 A1.1) Product analysis limit
Carbon (C) 0.06 – 0.10 0.01 under / over 0.05 – 0.11
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.045 0.010 over ≤ 0.055
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) ≤ 1.00 0.05 over ≤ 1.05
Chromium (Cr) 17.0 – 19.0 0.20 under / over 16.80 – 19.20
Nickel (Ni) 9.0 – 13.0 0.15 under / 0.20 over 8.85 – 13.20
Niobium (Nb) ≥ 8 × C, ≤ 1.10 0.05 over on max (Nb formula practice) max ≤ 1.15 product; min tied to heat C

UNCERTAIN: A480 product-tolerance digits for the Nb formula maximum — applied from sister-pack Nb practice; confirm A480 edition if product analysis is contractual.

Carbon, grain, and tensile snapshot — TP347 / TP347H / TP347HFG

Item TP347 (S34700) TP347H (S34709) TP347HFG (S34710)
C ≤ 0.08 0.04 – 0.10 0.06 – 0.10
Nb ≥ 10 × C, ≤ 1.10 ≥ 8 × C, ≤ 1.10 ≥ 8 × C, ≤ 1.10
Grain size (Table 3) no mandatory number No. 7 or coarser No. 7 – 10
Table 4 tensile, min 75 ksi [515 MPa] 75 ksi [515 MPa] 80 ksi [550 MPa]
Manufacture CF or HF CF or HF Cold-finished only

Dual TP347H/TP347HFG is not a casual chemistry path: the carbon floors differ (0.04 vs 0.06), the grain rules differ (“7 or coarser” vs “7–10”), the tensile floors differ (75 vs 80 ksi), and hot-finished TP347H cannot meet the HFG cold-finished-only manufacture rule. Dual TP347/TP347HFG is likewise blocked by carbon floor and grain/tensile/manufacture differences. Versus A213 TP321H, TP347HFG carries niobium rather than titanium and adds the fine-grain / Footnote I package.

When product analysis is ordered, finished tube may read C 0.05–0.11%, Mn ≤2.04%, P ≤0.055%, S ≤0.035%, Si ≤1.05%, Cr 16.80–19.20%, Ni 8.85–13.20%, and Nb max ≤1.15% with the formula minimum still tied to heat carbon. Put any tighter project carbon floor on the purchase order before the heat is selected — the 0.06% floor is intentional for this fine-grain H-grade row.

Mechanical Properties of A213 TP347HFG

ASTM A213 Table 4 sets the room-temperature tensile acceptance floor for TP347HFG at 80 ksi [550 MPa] tensile strength and 30 ksi [205 MPa] yield strength (0.2% offset), with elongation of 35% minimum in 2 in. or 50 mm. That tensile floor is 5 ksi higher than TP347 and TP347H (both 75 ksi). Hardness maximum is 192 HBW / 200 HV or 90 HRB, and hardness tests are part of lot acceptance under A213. Grain size must fall in ASTM No. 7 to 10 — a band with both a coarse bound (7) and a fine bound (10) — determined per heat-treatment lot under the ordered edition’s clause referencing ASTM E112. UNCERTAIN: how design-code creep-rupture allowables for fine-grain S34710 are framed relative to coarse-grain S34709 on a given Code edition — A213 publishes the grain band and tensile floors, not the allowables table.

Property TP347HFG requirement
Tensile strength, min (Table 4) 80 ksi [550 MPa]
Yield strength (0.2% offset), min (Table 4) 30 ksi [205 MPa]
Elongation in 2 in. or 50 mm, min (Table 4) 35%
Hardness, max (Table 4) 192 HBW / 200 HV or 90 HRB
Grain size ASTM No. 7 to 10 (per heat-treatment lot)

Source: ASTM A213/A213M Table 4 for TP347HFG / UNS S34710 and Table 3 grain-size column “7–10” (public specification PDF excerpt — _ref_a213.txt / A213–13). Mechanical property requirements do not apply to tubing smaller than 1/8 in. [3.2 mm] inside diameter or thinner than 0.015 in. [0.4 mm] wall. Flattening and flaring tests are also required on a lot basis.

A tensile-only MTC that omits grain size inside the 7–10 band, or that reports 75 ksi as if the heat were TP347H, is incomplete for TP347HFG. Ask for the E112 result and the 80 ksi tensile floor on the certificate before releasing the heat to fabrication. Do not accept a coarse-grain “7 or coarser” reading that sits outside the fine bound of 10 as HFG acceptance.

Dimensions and Tolerances

Dimensional supply for ASTM A213 TP347HFG is tube language — outside diameter × wall thickness (minimum wall or average wall) and, commercially, BWG / gauge — not ASME B36.19 pipe schedules as the primary size story. The sizes usually furnished under A213 run from about 1/8 in. [3.2 mm] inside diameter to 5 in. [127 mm] outside diameter, with minimum wall from about 0.015 to 0.500 in. [0.4 to 12.7 mm]; other diameters may be furnished when all other requirements are met. State on the purchase order whether wall is minimum or average — boiler and superheater datasheets almost always assume a minimum-wall reading.

Because TP347HFG shall be cold finished (A213 6.1), the dimensional route is the cold-finished A1016/A1016M window — not the wider hot-finished window available to TP347H. Cold-finished tubes commonly hold tighter OD control; permissible variations from a specified average wall for cold-finished tube are often summarized as ±10% of the specified average wall. Confirm the exact A1016 rows for the OD on the ordered edition.

Item Typical A213 TP347HFG dimensional practice
Product form Seamless cold-finished only (hot-finished not permitted for this grade under A213 6.1)
Usual size band ~1/8 in. [3.2 mm] ID to 5 in. [127 mm] OD; wall ~0.015–0.500 in. [0.4–12.7 mm] min (or average wall if PO says so)
Wall basis Minimum wall (default for boiler / superheater) or average wall when specified
OD / wall tolerances Per ASTM A1016/A1016M cold-finished rows; cold-finished average wall often ±10%
Length Cut lengths for boiler / superheater / HX bundles, or mill random lengths by agreement
Secondary size note ASME B36.19 schedules may appear only when a buyer asks for a pipe-schedule cross-reference — not as the primary A213 size callout

Put the cut list, design metal temperature context, and end preparation on the enquiry so mill lengths can be planned against the cold-finished-only rule. Minimum wall is a first-class A213 concept. If the datasheet actually wants hot-finished H-grade Nb tube, open A213 TP347H instead of forcing HFG into a hot-finished route it does not allow.

Equivalent Grades

Equivalence language around TP347HFG tube is especially risky because “fine-grain 347H” shop talk does not always map to UNS S34710. ASTM A213 Grade TP347HFG / UNS S34710 is the governing designation for this article; EN or JIS wrought names that point to general 347H families are not automatic substitutes on an A213 mill test certificate that must carry the HFG grain band, 80 ksi tensile floor, cold-finished-only manufacture, and Footnote I heat-treatment path. When a datasheet says “fine-grain 347H” or “347HFG,” confirm which product standard, UNS number, grain band, tensile floor, and manufacture route the mill will actually certify.

Designation Notes
ASTM A213 / A213M Grade TP347HFG Governing ASTM seamless boiler / HX tube product standard for this article
UNS S34710 Unified number listed in the stainless chemistry table — distinct from S34709 (TP347H)
ASME SA-213 TP347HFG Separate ASME Code Book adoption — dual-mark only when the PO asks
Shop “fine-grain 347H” Not a substitute designation — confirm S34710, grain 7–10, 80 ksi, cold-finished only
Related plate A240 / SA240 flat product in related Nb-stabilized families — order plate and tube under their own product standards; do not assume plate “347H” equals tube HFG

Dual A213/SA-213 marking is a purchase-order option, not a claim that the two standards are one document. Compare TP347H and TP347 on their own ASTM A213 pages before accepting a familiar “347H” PMI reading as HFG paperwork.

Heat Treatment and Delivery Condition

TP347HFG under ASTM A213 is furnished solution treated at 2150 °F [1175 °C] (public Table 3), then quenched in water or cooled rapidly by other means, with Footnote F on the quench capability. Grain size after heat treatment must fall in ASTM No. 7 to 10 for the heat-treatment lot. Footnote I on the TP347HFG heat-treatment row requires that solution treatment be preceded by a softening heat treatment prior to cold working: the softening temperature shall be at least 90 °F [50 °C] higher than the solution heat treatment temperature, which Footnote I states shall be at 2150 °F [1180 °C] minimum. UNCERTAIN: the SI conversion difference between the Table 3 bracket [1175 °C] and the Footnote I body [1180 °C] — confirm the ordered edition wording and mill practice before treating either digit as the sole contractual temperature.

Clause 6.1 states that Grade TP347HFG shall be cold finished — so the Footnote I softening-before-cold-work sequence is not optional process folklore; it is part of how the grade is made. Hot-finished delivery is not an A213 option for this UNS row. The public A213–13 Supplementary Requirement S2 list includes TP347 and TP347H but does not list TP347HFG in the excerpt used here — UNCERTAIN whether a later edition adds HFG to S2; do not assume S2 from the TP347H listing alone. Write any stabilization or IGC Supplementary Requirement explicitly on the purchase order.

Delivery condition for SHH STEEL TP347HFG is cold-finished, solution annealed (after the Footnote I softening sequence) and pickled (or bright annealed by agreement), with softening temperature, solution temperature, quench method, niobium result, and grain-size result inside 7–10 stated on the EN 10204 3.1 certificate. For coarse-grain H-grade Nb without the HFG package open A213 TP347H; for non-H Nb open A213 TP347.

Corrosion Resistance

TP347HFG’s chromium-rich passive film and niobium stabilization handle the oxidizing steam-side and many water-side duties typical of boiler and superheater service, with niobium tying up carbon during sensitizing thermal cycles. The fine-grain band and higher carbon floor are written for elevated-temperature mechanical behavior, not as a wet-chloride corrosion upgrade. In chloride-bearing cooling waters and many process exchangers, pitting and crevice attack become limiting, and buyers usually step to molybdenum-bearing grades rather than stretching fine-grain H-grade Nb-stabilized 18-8 into wet corrosive service.

ASTM A213 itself does not publish a corrosion-rate table for TP347HFG; selection remains engineering judgment against fluid, temperature, velocity, and inspection philosophy inside the boiler or exchanger. When a specification calls for ASTM A262 Practice E, write Supplementary Requirement S4 onto the purchase order and confirm with the mill whether a stabilization step is needed for the HFG heat-treatment path — the public S2 list in the A213–13 excerpt does not name TP347HFG, so do not invent S2 applicability from the TP347H row. SHH STEEL will not market TP347HFG as a wet-service upgrade over A213 TP304L — the HFG designation is about fine-grain creep-range framing, cold-finished manufacture, and the 80 ksi tensile floor, not about better aqueous chloride resistance.

Applications of A213 TP347HFG Tube

TP347HFG seamless tube under A213 is chosen for creep-range boiler, superheater, and reheater service where the design code’s elevated-temperature allowables for fine-grain S34710, the 0.06–0.10% carbon band, niobium stabilization, the ASTM No. 7–10 grain band, the 80 ksi tensile floor, and cold-finished manufacture earn their keep. It is the wrong default when the datasheet only says “347H” without fine-grain language, and it is not a hot-finished product. UNCERTAIN: project-specific creep-life framing that cites “fine grain” without naming S34710 — confirm the UNS and A213 grade on the datasheet before ordering. The table below pairs typical application areas with a selection note.

Application area Typical use of TP347HFG tube Selection note
Superheater / reheater (fine-grain spec) Cold-finished A213 tube where S34710, grain 7–10, and 80 ksi are specified Do not substitute TP347H coarse-grain stock
High-temperature boiler tube with HFG callout Creep-range steam tubing ordered explicitly to A213 TP347HFG Confirm cold-finished-only and Footnote I path on the MTC
“Fine-grain 347H” datasheets Only when the PO maps shop language to UNS S34710 If the datasheet means S34709, open TP347H instead
Hot-finished H-grade Nb tube Not an HFG application Open A213 TP347H
Wet chloride HX Not a first-choice HFG application Prefer Mo-bearing or L grades

For coarse-grain Nb H-grade open A213 TP347H; for non-H Nb open A213 TP347; for titanium H-grade open A213 TP321H on the A213/A213M hub.

Weldability

TP347HFG tube welds with matching or near-matching niobium-bearing austenitic filler for tube-to-tubesheet joints, attachment welds, and fabrication joins. Common practice uses ER347 / ER347H (or equivalent covered electrodes) under a qualified WPS so weld-metal niobium and carbon support elevated-temperature stabilized service; many fabricators avoid defaulting to ER308L when the base tube is fine-grain H-grade Nb-stabilized and the design allowables assume H-grade carbon with the HFG grain band. Heat input control, interpass limits, and post-weld cleaning remain the fabricator’s responsibility under the applicable boiler or pressure-vessel code — A213 governs the seamless tube product, not the field or shop weld procedure. UNCERTAIN: whether a project WPS written for coarse-grain TP347H needs re-qualification when the base metal is S34710 — that is a fabricator/Code question, not an A213 product-clause answer.

Because A213 TP347HFG is seamless and cold-finished only, there is no mill longitudinal weld to radiograph the way welded pipe standards describe. Focus inspection language on tube integrity (hydro or NDE of each length), tube-to-tubesheet joint quality, grain-size inside 7–10 and niobium documentation on the base metal, and any contractual corrosion test. Specify end preparation and surface finish on the tube PO when orbital or clean-service joins are planned.

Surface Finishes

Standard mill delivery for ASTM A213 TP347HFG is cold-finished, solution annealed (after Footnote I softening) and pickled, leaving a clean matte finish suitable for most boiler and heat-exchanger tube duty. Bright annealing under protective atmosphere produces a smoother reflective surface used on some clean-process lines and must be called out because it changes the heat-treatment route — and must still deliver the required grain size inside 7–10 and niobium chemistry. Light polish or specified Ra on the bore or OD is a commercial or service-center operation on top of A213 product, not automatic with the grade stamp.

When a fouling-sensitive exchanger specification quotes an Ra maximum on the bore, put it on the tube purchase order with its own acceptance language and sampling plan. SHH STEEL stencils grade, cold-finished identity, heat treatment, and (on request) HFG / Nb identity as standard requirements; polish, special OD grind, and passivation after fabrication remain commercial extras unless the contract says otherwise. Order end preparation together with finish so receiving inspection shares one acceptance language.

Inspection and Testing

Base ASTM A213 testing for TP347HFG includes heat analysis (carbon inside 0.06–0.10%, niobium meeting ≥8 × C ≤1.10%), tension tests to the Table 4 floors (80/30 ksi), hardness tests to the Table 4 maximum (192 HBW / 90 HRB), grain-size determination (ASTM No. 7 to 10) per heat-treatment lot, flattening and flaring tests on a lot basis, and either hydrostatic testing or nondestructive electric testing of each length. The manufacturer may choose hydro versus NDE unless the purchase order fixes the method. Marking includes the ASTM designation, grade, size, heat number, and other clause-required data. Confirm cold-finished manufacture on the MTC — hot-finished is not permitted for this grade.

Supplementary Requirements commonly added on TP347HFG tube orders are summarized below. Invoke them by number or clear purchase-order wording; mills will not assume product analysis, IGC testing, or “fine-grain” reporting detail from a verbal “full certs” note. UNCERTAIN: S2 applicability to TP347HFG — not listed in the public A213–13 S2 excerpt; write stabilization temperature explicitly if required.

Option Purpose
Product analysis Confirms chemistry on finished tube — useful when carbon sits near the 0.06% floor or 0.10% ceiling
Grain-size reporting (7–10) Ensures E112 result appears on the MTC inside the fine-grain band
S4 intergranular corrosion A262 Practice E when ordered — confirm any needed stabilization step with the mill
Explicit stabilization anneal PO language if required — do not assume S2 from the TP347H listing alone
Minimum vs average wall States which wall basis the size callout uses
Fixed hydro or NDE method Removes manufacturer’s option when the end user mandates one route
Third-party inspection / EN 10204 3.2 Witnessed testing and certificate when the project requires it

Ask the mill to state lot identity clearly on the certificate so hardness, tension, niobium, Footnote I temperatures, and grain-size specimens map cleanly to the bundle you receive. A tensile-only MTC without grain size inside 7–10, or a 75 ksi tensile reading offered as HFG, is incomplete.

Packaging and Shipping

TP347HFG tube leaves SHH STEEL bundled, capped or end-protected, and tagged for export or domestic delivery according to the length mix and bend form on the order. Bundle tags repeat the ASTM A213 grade (including HFG identity), OD × wall (or BWG), heat number, and PO reference so site receiving can check the shipment without opening every certificate packet first. U-bent tubes need extra cradle or case protection so bend radii and legs are not distorted in transit.

Export packing can be bare bundles, wrapped bundles, or wooden-cased lengths for bright-annealed, polished, or small-bore material. We ship under the Incoterms on the order acknowledgement — FOB, CFR, CIF, EXW, or other agreed terms. Inland trucking, bilingual destination marks, or project color coding for bundle tags should be stated on the enquiry beside the metallurgical notes.

Why Choose SHH STEEL

SHH STEEL treats ASTM A213 TP347HFG as a product standard with enforceable chemistry (carbon 0.06–0.10%, niobium formula), tensile (80 ksi floor), hardness, fine-grain band (7–10), cold-finished-only manufacture, Footnote I heat-treatment sequence, and marking rules — not as a catalogue nickname for “any fine-grain 347H tube.” The MTC reports the full ladle chemistry including niobium against 8 × C, the Table 4 tensile/hardness set (80/30 ksi, 192 HBW / 90 HRB), and the grain-size result inside 7–10; the stencil carries seamless cold-finished tube identity under A213; and dual A213/SA-213 marking is offered only when requested.

We keep the fine-grain conversation honest for boiler and HX duty. If the datasheet only needs coarse-grain H-grade Nb without the HFG package, we open A213 TP347H. If H-grade carbon and grain size are not required, we open A213 TP347. If titanium is preferred, we open A213 TP321H. If hot-finished delivery is mandatory, HFG is the wrong grade — we say so and open TP347H. The A213/A213M hub is organized grade by grade under ASTM, seamless tube only.

Lead times combine near-term cold-finished stock lengths with mill schedules; we say which is which on the quotation. Cut-to-length, U-bending, polish, and third-party inspection are defined extras. The tube that arrives should match the ASTM HFG callout the engineer wrote, with paperwork a third-party inspector can read without translation.

Supply Capability

SHH STEEL can supply ASTM A213 TP347HFG stainless steel tube against the edition named on your enquiry — cold-finished only. The capability table below summarizes the sizes, finishes, and documents we regularly quote for this grade, followed by the Stock / Available sizes map buyers ask for when they need a quick sense of what to enquire against for fine-grain Nb-stabilized boiler and superheater duty.

Item SHH STEEL capability for TP347HFG
Standard ASTM A213 / A213M (dual SA-213 marking on request) Grade TP347HFG / UNS S34710
Product form Seamless cold-finished only (A213 6.1) — not hot-finished
Size Typical OD × min wall (or average wall) in the A213 usual band; other diameters by agreement
Wall / gauge Minimum wall or average wall; BWG / gauge callouts accepted on enquiry
Length Cut-to-length for boiler / superheater / HX bundles; mill random by agreement; U-bends on enquiry
Finish Annealed and pickled after Footnote I path; bright annealed or light polish by agreement
Testing Tension (80/30 ksi), hardness (max 192 HBW / 90 HRB), grain size No. 7–10, Nb vs 8×C, flattening, flaring, hydro or NDE per length; full ladle chemistry on MTC; product analysis / S4 on order
Documents EN 10204 3.1 with full ladle chemistry, Nb, Footnote I temperatures, and grain-size result; third-party inspection / 3.2 on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

Stock / Available sizes

SHH STEEL quotes TP347HFG tube against a practical stock-and-mill enquiry range rather than a frozen warehouse SKU list. The sizes below are OD × wall / BWG combinations buyers most often request for fine-grain Nb-stabilized H-grade boiler and superheater tube; availability of any single line on a given week depends on mill drawing and our inbound cold-finished schedule, so treat the table as a supply map for enquiry — not a guarantee of floor tonnage.

Item Typical stock / enquiry range for TP347HFG
Outside diameter 25.4, 31.8, 38.1, 44.5, 50.8, 63.5, 76.2 mm (and other boiler/HX ODs on enquiry; up through the usual A213 ~5 in. [127 mm] band)
Wall / BWG BWG 10–16 class walls and metric min-wall equivalents; heavier walls for high-pressure boiler duty by agreement
Common OD × wall examples 31.8 × 2.77 mm; 38.1 × 3.05 mm; 50.8 × 3.05 mm; 50.8 × 3.40 mm; 63.5 × 3.40 mm — illustrative boiler/HX sizes, confirm min vs average wall
Length Cut lengths for boiler / superheater / exchanger bundles; U-bends and straight random lengths on enquiry
Special Non-standard OD/wall, bright anneal, dual A213/SA-213 marking, explicit stabilization anneal, third-party grain-size witness — confirm on enquiry before the heat is reserved

When you send an enquiry, list OD × wall (or BWG), wall basis (minimum or average), quantity or cut list, required marking (A213 alone or dual A213/SA-213), confirmation that cold-finished HFG is intended (not hot-finished TP347H), and any Supplementary Requirements (product analysis, S4, explicit stabilization). We reply with what we can ship from near-term cold-finished stock versus what needs a mill run, without inventing fake warehouse codes or tonnage claims.

Send the size list, quantity or cut lengths, required marking, Supplementary Requirements, and destination on one enquiry. We will confirm chemistry (including the 0.06–0.10% carbon band and Nb formula), tensile (80 ksi), hardness, grain size inside 7–10, and cold-finished manufacture against the stainless chemistry table, Table 4, and Table 3, state what ships from near-term availability versus mill production, and keep the offer aligned with ASTM A213 / A213M. Related grades such as A213 TP347H, A213 TP347, and A213 TP321H sit on the same hub when the datasheet steps beyond TP347HFG.

FAQ

Is ASTM A213 the same as ASME SA-213 for TP347HFG?
No. ASTM A213 / A213M is the ASTM International product specification for seamless boiler, superheater, and heat-exchanger tubes; ASME SA-213 / SA-213M is the separate ASME Code Book adoption of that grade text. Chemistry, tensile, hardness, niobium formula, fine-grain band, and cold-finished-only rules align closely for a given referenced edition, but they remain two independent standards. Dual-mark A213/SA-213 tube only when the purchase order asks for both names on the stencil and MTC.
Does ASTM A213 TP347HFG include welded, HCW, or hot-finished tube?
No. ASTM A213 covers seamless tube only — no WLD or HCW manufacturing type. For TP347HFG specifically, clause 6.1 further requires cold-finished manufacture; hot-finished delivery is not an A213 option for UNS S34710. If you need hot-finished H-grade Nb tube, open TP347H instead of forcing an HFG stamp onto a hot-finished route.
How does TP347HFG differ from TP347H under ASTM A213?
TP347HFG uses carbon 0.06–0.10% (higher floor), grain size ASTM No. 7 to 10, Table 4 tensile 80 ksi [550 MPa], cold-finished manufacture only, and the Footnote I softening-plus-2150 °F solution path. TP347H uses carbon 0.04–0.10%, grain size No. 7 or coarser, tensile 75 ksi, either cold-finished or hot-finished, and finish-route solution temperatures of 2000 / 1925 °F. Both share Nb ≥8 × C ≤1.10%. Do not treat HFG as a synonym stamp for ordinary TP347H on the MTC.
What is the UNS number and chemistry of ASTM A213 TP347HFG?
TP347HFG is UNS S34710. Melting limits include carbon 0.06–0.10%, manganese ≤2.00%, phosphorus ≤0.045%, sulfur ≤0.030%, silicon ≤1.00%, chromium 17.0–19.0%, nickel 9.0–13.0%, and niobium ≥8 × C ≤1.10%, with molybdenum, nitrogen, and titanium as no-requirement ellipses. Product-analysis limits apply only when ordered. Confirm the ordered A213 edition for the exact stainless-table number.
Does A213 Table 4 set a hardness and higher tensile floor for TP347HFG?
Yes. Table 4 for TP347HFG lists tensile strength 80 ksi [550 MPa] minimum — five ksi above TP347H — with yield 30 ksi [205 MPa], elongation 35%, and hardness maximum 192 HBW / 200 HV or 90 HRB. Hardness tests are part of lot acceptance under A213. Grain size No. 7 to 10 sits beside those Table 4 numbers as an HFG acceptance item. A 75 ksi tensile reading is not HFG acceptance.
Why does ASTM A213 control grain size to No. 7–10 on TP347HFG?
The 7–10 band is the fine-grain control that distinguishes HFG from coarse-grain TP347H ("7 or coarser"). It supports the elevated-temperature fine-grain framing buyers specify for S34710, sitting beside niobium stabilization and the higher tensile floor. A tensile-only MTC without an E112 result inside 7–10 is incomplete. Ask the mill to report grain size per heat-treatment lot on the EN 10204 3.1 certificate before releasing the heat.
What does Footnote I require for TP347HFG heat treatment?
Footnote I requires a softening heat treatment before cold working, at least 90 °F [50 °C] above the solution heat-treatment temperature, which Footnote I states shall be 2150 °F [1180 °C] minimum. Table 3 prints 2150 °F [1175 °C] for the solution row. UNCERTAIN: reconcile the [1175] vs [1180] SI bracket on the ordered edition. Ask the mill to state both softening and solution temperatures on the MTC.
Is Supplementary Requirement S2 listed for TP347HFG?
The public A213–13 S2 excerpt lists TP347 and TP347H among grades that shall receive a stabilization heat treatment when S2 is specified, but does not name TP347HFG in that list. UNCERTAIN whether a later edition adds HFG. Do not assume S2 from the TP347H listing alone — write any required stabilization temperature explicitly on the purchase order and confirm with the mill.
Can I substitute TP347H stock for a TP347HFG datasheet?
Usually no. Carbon floor, grain band, tensile floor, manufacture route (hot-finished TP347H vs cold-finished-only HFG), and heat-treatment path all differ. A coarse-grain TP347H MTC does not clear ASTM No. 7–10 or the 80 ksi tensile floor. Spell UNS S34710 and grade TP347HFG on the enquiry; if the datasheet only meant coarse-grain 347H, open TP347H deliberately rather than stretching labels.
Minimum wall vs average wall — which should I order for A213 TP347HFG?
Order minimum wall when the boiler or superheater datasheet is written around a guaranteed minimum thickness after tolerance — the usual practice for A213 H-grade tube. Order average wall only when the purchase order explicitly allows average-wall product and the designer has accepted that basis. Put the wall basis on the enquiry before the mill selects A1016 cold-finished tolerance tables.
Is TP347HFG a good choice for wet corrosive heat-exchanger service?
Usually no as a first choice for chloride-rich aqueous duty. The higher carbon floor and absence of molybdenum mean pitting and crevice attack can limit life; niobium helps IGC when properly applied but does not replace Mo for chlorides. Prefer TP304L or TP316L for wet as-welded service; reserve TP347HFG for fine-grain creep-range boiler and superheater framing where the HFG package earns its keep.
Hydrostatic test vs NDE — which do I get on TP347HFG tube?
ASTM A213 requires each tube to be hydrostatically tested or nondestructively electrically tested. The manufacturer may choose the method unless the purchase order fixes one. Neither route is an informal upgrade over the other inside the product standard. State the preferred method on the enquiry if your end user or inspector mandates hydro only or a named NDE technique.

Conclusion

ASTM A213 TP347HFG / UNS S34710 is the fine-grain, niobium-stabilized, cold-finished-only seamless stainless steel tube grade for creep-range boiler, superheater, and heat-exchanger service when elevated-temperature fine-grain framing, a 0.06–0.10% carbon band, niobium ≥8 × C ≤1.10%, ASTM grain size No. 7 to 10, Table 4 tensile 80 ksi [550 MPa], and the Footnote I softening-plus-2150 °F solution path share one datasheet. SHH STEEL supplies cold-finished seamless tube in the usual OD × wall / BWG band, solution annealed after the Footnote I sequence, tested to Table 4 tensile and hardness limits with niobium and grain size inside 7–10 reported, and documented on EN 10204 3.1 certificates — with dual SA-213 marking only when the order asks for that separate ASME standard. For sister grades and stock-oriented size discussions, start from the A213/A213M hub, then send your OD × wall list, wall basis, confirmation of cold-finished HFG (not hot-finished TP347H), and Nb / grain-size requirements so we can align mill and near-term availability to the ASTM callout.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X