ASME SA213 UNS S30815 Stainless Steel Tube | ASME SA213 Stainless Steel - SHH STEEL

ASME SA213 UNS S30815 Stainless Steel Tube

ASME SA213 UNS S30815 Ce–N high-temperature austenitic seamless boiler, superheater and heat-exchanger tube — commercially 253 MA class — C 0.05–0.10%, Si 1.40–2.00%, Mn ≤0.80%, Cr 20.0–22.0%, Ni 10.0–12.0%, N 0.14–0.20%, Ce 0.03–0.08%, Table 4 87/45 ksi with elongation 40% min, hardness max 217 HBW / 95 HRB, 1920 °F solution anneal. No TP letter — order by UNS. SHH STEEL supplies cold-finished and hot-finished seamless tube with EN 10204 3.1 MTCs that report Ce and N together.
Grade
UNS S30815 (no TP letter — Ce–N high-temperature austenitic)
Standard
ASME SA213 / SA213M
Product form
Seamless boiler / superheater / heat-exchanger tube (cold-finished and hot-finished)
Size
Typical OD × min wall (or average wall) within ~1/8 in. [3.2 mm] ID to 5 in. [127 mm] OD and ~0.015–0.500 in. [0.4–12.7 mm] wall; other diameters by agreement
Share:
Overview
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA213 UNS S30815 Stainless Steel Tube

ASME SA-213 / SA-213M is the ASME Boiler and Pressure Vessel Code Book adoption of the seamless ferritic and austenitic alloy-steel boiler, superheater, and heat-exchanger tube product text. When Code-stamped boilers, process heaters, or heat exchangers invoke that adoption by name, SA-213 is the governing product standard for this cerium–nitrogen high-temperature austenitic tube — written as its own Code Book line, not as a merged synonym of ASTM A213. Begin from SA213/SA213M when the enquiry is Code-led.

UNS S30815 sits in the stainless chemistry table without a TP grade letter (Footnote C practice). Melting carbon sits in a 0.05–0.10% band, silicon in a deliberate 1.40–2.00% window, manganese capped tightly at ≤0.80%, chromium at 20.0–22.0%, nickel at 10.0–12.0%, nitrogen at 0.14–0.20%, and cerium at 0.03–0.08%, with phosphorus ≤0.040% and sulfur ≤0.030%. Molybdenum, niobium, and titanium have no requirement on the public row. Table 4 sets tensile at 87 ksi [600 MPa] / 45 ksi [310 MPa] with elongation 40% minimum and hardness max 217 HBW / 95 HRB. Buyers who write “253 MA” on a bill of materials still need to name SA-213 UNS S30815 on the purchase order so the mill applies the tube product standard, minimum-wall rules, and the Ce/N windows together. This is not a dual stamp of SA213 TP309S or of the high-Si Al grade SA213 UNS S30615.

SHH STEEL can supply ASME SA213 UNS S30815 as seamless cold-finished and hot-finished tube in the usual OD × wall / BWG band, with EN 10204 3.1 certificates that report cerium and nitrogen together with the 87/45 ksi tensile set, 40% elongation, and hardness. Dual SA-213/A213 marking is added only when the purchase order asks; the live twin is A213 UNS S30815.

Shop names include “S30815,” “253 MA,” and “Ce–N 21Cr.” Helpful for routing; the commercial 253 MA trademark nickname does not replace UNS S30815 on the MTC. The purchase order should still carry ASME SA-213 UNS S30815, wall basis, OD × wall or BWG, finish route, and any Supplementary Requirements when needed. Sister SA213 pages include SA213 TP309S, SA213 TP310S, SA213 UNS S30615, and SA213 TP XM-15. Seamless only — no Manufacturing Types (SML / WLD / HCW) product-form split on this page.

Chemical Composition of SA213 UNS S30815

Two chemistry layers matter for UNS S30815 under ASME SA-213. Melting analysis is mandatory for every heat; product analysis on finished tube applies only when Supplementary Requirement wording or the purchase order invokes it through the general requirements (commonly ASTM A1016/A1016M), with tolerances typically from ASTM A480/A480M Table A1.1. The defining package for a reviewer is silicon 1.40–2.00% together with nitrogen 0.14–0.20%, cerium 0.03–0.08%, chromium 20.0–22.0%, and nickel 10.0–12.0% — plus the tight manganese ceiling ≤0.80% that most TP304-family rows do not share. Carbon sits in a 0.05–0.10% band. Nitrogen analysis method is by agreement (Footnote B). There is no mandatory Mo, Nb, Ti, or Al band on the public row.

The tables below reproduce the melt limits for UNS S30815, the product-analysis limits from A480 Table A1.1 practice, and a short Ce/N snapshot against TP309S and related high-temperature grades. Later SA-213 / A213 editions place austenitic stainless grades in Table 2 (older editions used Table 1); confirm the ordered edition on the purchase order. UNCERTAIN: exact edition year and stainless chem table number on the ordered Code Book text; rare-earth (Ce) product-tolerance digits if A480 is contractual.

Melting analysis (heat / ladle analysis)

Element UNS S30815 melting analysis
Carbon (C) 0.05 – 0.10
Manganese (Mn) ≤ 0.80
Phosphorus (P) ≤ 0.040
Sulfur (S) ≤ 0.030
Silicon (Si) 1.40 – 2.00
Chromium (Cr) 20.0 – 22.0
Nickel (Ni) 10.0 – 12.0
Molybdenum (Mo) … (no requirement)
Nitrogen (N) 0.14 – 0.20
Niobium (Nb) … (no requirement)
Titanium (Ti) … (no requirement)
Cerium (Ce) 0.03 – 0.08

Source: public SA-213 / A213 stainless chemistry table for UNS S30815 (same grade text family; public A213/A213M − 13 excerpt). Cerium and nitrogen must both appear on the certificate; an MTC that reports only Cr–Ni–Si without Ce and N is incomplete for S30815. Where ellipses appear, the ordered edition sets no requirement for that element.

Product analysis — A480/A480M Table A1.1 tolerances applied

Element Melting Tolerance (A480 A1.1) Product analysis limit
Carbon (C) 0.05 – 0.10 0.01 under / over 0.04 – 0.11
Manganese (Mn) ≤ 0.80 0.03 over ≤ 0.83
Phosphorus (P) ≤ 0.040 0.010 over ≤ 0.050
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) 1.40 – 2.00 0.05 under / over 1.35 – 2.05
Chromium (Cr) 20.0 – 22.0 0.25 under / over 19.75 – 22.25
Nickel (Ni) 10.0 – 12.0 0.15 under / over 9.85 – 12.15
Nitrogen (N) 0.14 – 0.20 0.01 under / 0.02 over 0.13 – 0.22
Cerium (Ce) 0.03 – 0.08 edition-dependent rare-earth tolerance confirm A480 edition if contractual (UNCERTAIN)

Product analysis is not automatic — order it when the project needs finished-tube chemistry, especially the cerium and nitrogen windows. Read Ce, N, and Si first: cerium supports oxide-scale adherence at elevated temperature; nitrogen strengthens and helps oxidation resistance; silicon adds further scaling resistance.

Ce / N snapshot — TP309S / S30815 / S30615

Element TP309S (S30908) S30815 S30615
Si ≤ 1.00 1.40 – 2.00 3.2 – 4.0
N none required 0.14 – 0.20 none required
Ce / Al none required Ce 0.03 – 0.08 Al 0.8 – 1.5
Mn ≤ 2.00 ≤ 0.80 ≤ 2.00
Cr 22.0 – 24.0 20.0 – 22.0 17.0 – 19.5

Reading tip: a heat that clears TP309S still fails S30815 if cerium and nitrogen are absent or manganese sits above 0.80%. Do not accept a verbal “253 MA” shop note as proof that the MTC prints S30815 with the Ce and N windows satisfied.

Mechanical Properties of SA213 UNS S30815

Table 4 of the public SA-213 / A213 grade text family sets UNS S30815 tensile strength at 87 ksi [600 MPa] minimum and yield (0.2% offset) at 45 ksi [310 MPa] minimum — a yield floor above XM-15’s 30 ksi and even above S30615’s 40 ksi under the same product standard. Elongation in 2 in. or 50 mm is 40% minimum (higher than the 35% commodity austenitic floor), and hardness is capped at 217 HBW or 95 HRB. Nitrogen strengthening is a large part of why the yield and hardness rows sit above classic 18-8 / 309S levels.

Property UNS S30815 requirement (Table 4)
Tensile strength, min 87 ksi [600 MPa]
Yield strength (0.2% offset), min 45 ksi [310 MPa]
Elongation in 2 in. or 50 mm, min 40%
Hardness, max 217 HBW or 95 HRB
Grain size No mandatory ASTM grain-size number

S30815 has no mandatory ASTM grain-size number in the heat-treatment column. If a project datasheet asks for an E112 grain-size report, put that supplementary requirement on the purchase order rather than assuming base SA-213 includes it. Mechanical property requirements generally do not apply to tubing smaller than 1/8 in. [3.2 mm] ID or thinner than 0.015 in. [0.4 mm] wall. Flattening and flaring follow the general requirements for the ordered size; hydrostatic or nondestructive examination follows the path selected on the PO. Do not accept a TP309S certificate as S30815 clearance — Ce, N, the Mn ≤0.80% ceiling, and the 87/45 ksi pair must all match.

Dimensions and Tolerances

Dimensional supply for ASME SA213 UNS S30815 is tube language — outside diameter × wall thickness (minimum wall or average wall) and, commercially, BWG / gauge — not ASME B36.19 pipe schedules as the primary size story. Usual SA-213 sizes run from about 1/8 in. [3.2 mm] inside diameter to 5 in. [127 mm] outside diameter, with minimum wall from about 0.015 to 0.500 in. [0.4 to 12.7 mm]; other diameters may be furnished when all other requirements are met.

Furnace, boiler, and heat-exchanger datasheets that pick Ce–N S30815 usually assume minimum wall — state wall basis on the purchase order. Outside-diameter and wall variations follow the general requirements invoked by SA-213 (commonly ASTM A1016/A1016M). The Ce/N package does not change the dimensional tolerance tables; it changes which heat clears the grade stamp.

Item Typical SA213 UNS S30815 dimensional practice
Product form Seamless only (cold-finished or hot-finished)
Usual size band ~1/8 in. [3.2 mm] ID to 5 in. [127 mm] OD; wall ~0.015–0.500 in. [0.4–12.7 mm]
Wall basis Minimum wall (common for furnace / HX datasheets) or average wall if PO says so
OD / wall tolerance Per general requirements (commonly A1016/A1016M) for the ordered finish
Length Straight random / cut-to-length; U-bend by agreement

BWG / gauge callouts are accepted on enquiry; certificates should still show OD and wall in inch or millimetre units. U-bends and polished ID finishes are commercial options — they do not replace the cerium and nitrogen window checks.

Equivalent Grades

Equivalence talk for S30815 should start from the Code Book product standard and the UNS, not from the commercial 253 MA nickname. ASME SA-213 UNS S30815 is the governing designation on this page. ASTM A213 UNS S30815 is the separate ASTM twin used when dual marking or a non-Code purchase is agreed — it is not a substitute lead standard for an SA-213 order. Related high-temperature grades (TP309S, S30615, TP310S, XM-15) are sister options under the same hub family, not automatic dual stamps.

Designation Notes
ASME SA-213 / SA-213M UNS S30815 Governing Code Book seamless boiler / HX tube product standard for this article
UNS S30815 Unified number — no TP letter (Footnote C)
253 MA (commercial) Shop / trademark name for the Ce–N chemistry family — does not replace S30815 on the MTC
ASTM A213 UNS S30815 Separate ASTM product specification — dual-mark only when the PO asks; twin page A213 UNS S30815
Related 309-family SA213 TP309S — similar Cr band, no Ce/N package
Related high-Si Al grade SA213 UNS S30615 — Si–Al story, not Ce–N
Related plate A240 / SA240 flat product in related high-temperature families — order plate and tube under their own standards

Hub entry point: SA213/SA213M. When a bill of materials only says “253 MA,” ask whether Ce 0.03–0.08% and N 0.14–0.20% are actually required before shipping S30815 or a TP309S alternative.

Heat Treatment and Delivery Condition

UNS S30815 under ASME SA-213 is furnished solution treated at a minimum of 1920 °F [1050 °C], then quenched in water or cooled rapidly by other means. That anneal temperature sits slightly above the 1900 °F commodity austenitic minimum used for many TP304 / TP309S rows — do not apply a generic “solution anneal 1900 °F” stamp to an S30815 heat without checking the ordered edition. Public Table 3 for S30815 does not print a mandatory grain-size number (ellipsis), so H-grade grain-size framing does not apply.

Cold-finished versus hot-finished is a process and dimensional route, not a substitute for the anneal. Ce–N austenitics need a thorough solution treatment so nitrogen stays in solution and cerium-supported scale behaviour is not compromised by incomplete anneal. Delivery condition for SHH STEEL S30815 is solution annealed and pickled (or bright annealed by agreement), with anneal temperature and quench method on the EN 10204 3.1 certificate. Straightening, cutting, and end finishing follow heat treatment.

UNCERTAIN: confirm ordered-edition footnote attachment near the S30815 heat-treatment row (public OCR does not clearly show Footnote F on that line the way S30615 does). If a later edition attaches quench / A262 capability language, follow the ordered text rather than inventing S4 test obligations that the edition does not require. If a project datasheet asks for an E112 grain-size report, put that supplementary requirement on the purchase order.

Corrosion Resistance

S30815 under ASME SA-213 is selected primarily for high-temperature oxidation and scaling resistance associated with the Ce–N–Si package — furnace, process-heater, and elevated-temperature HX framing — not as a general wet-chloride upgrade over TP316. Cerium supports oxide-scale adherence; nitrogen strengthens and contributes to oxidation resistance; silicon adds further scaling resistance relative to low-silicon 309S in many dry or mildly oxidizing services.

Where a datasheet mixes “253 MA” with wet process condensates or chloride deposits, ask whether the service is actually looking for a molybdenum-bearing or duplex tube instead of a Ce–N high-temperature austenitic. SHH STEEL will not treat a chromium PMI peak alone as proof of aqueous corrosion suitability — chemistry, heat treatment, and the intended medium have to be read together. For high-Si Al framing without cerium, open SA213 UNS S30615.

Applications of SA213 UNS S30815 Tube

Typical ASME SA213 UNS S30815 placements are Code-stamped boiler, superheater, process-heater, and heat-exchanger tubes where the material list names S30815 or explicitly requires the Ce–N package with Si 1.40–2.00% — not generic “309S,” “310,” or “high-Si” replacements. Furnace coils and high-temperature HX bundles that already distinguish 253 MA-class chemistry from TP309S are the natural fit.

When the enquiry only says “253 MA” without UNS language, confirm whether the buyer actually needs SA213 TP309S, SA213 TP310S, or the high-Si Al grade before substituting. SHH STEEL quotes S30815 when the enquiry names the UNS or the Ce/N package explicitly.

Weldability

S30815 welds as a Ce–N high-temperature austenitic. Filler selection should respect the elevated silicon, nitrogen, and cerium rather than copying a plain ER309 procedure without review. Matching or near-matching austenitic fillers qualified for the 253 MA-class chemistry are the usual starting point; confirm chemistry against the WPS when the project treats Ce/N as contractual on the weld metal as well as the tube.

Autogenous welds and thin-wall HX joints need heat-input control to protect the as-annealed condition near the HAZ. Post-weld heat treatment is not a default SA-213 requirement for this grade — if the vessel code or the buyer wants a separate resolution anneal after welding, write that as a negotiated step. SHH STEEL can coordinate weld coupons when the PO asks.

Surface Finishes

Standard mill delivery for ASME SA213 UNS S30815 is solution annealed and pickled, leaving a clean matte finish suitable for furnace, boiler, and heat-exchanger tube duty. Bright annealing is available by agreement when OD appearance or polish steps favor it.

ID/OD polish and U-bend conditioning are commercial additions — they do not replace the cerium and nitrogen window checks. End caps and dry export packaging matter more than paint on pickled stainless. SHH STEEL notes the ordered surface route on the packing list and aligns it with the MTC finish description for receiving inspection.

Inspection and Testing

Base ASME SA-213 testing for UNS S30815 includes heat analysis (C 0.05–0.10%, Si 1.40–2.00%, Mn ≤0.80%, Cr 20.0–22.0%, Ni 10.0–12.0%, N 0.14–0.20%, Ce 0.03–0.08%, P ≤0.040%, S ≤0.030%), tension tests to the 87/45 ksi floors with 40% elongation, hardness to 217 HBW / 95 HRB, and flattening / flaring tests for the ordered size. Hydrostatic testing or NDE follows the path selected on the purchase order.

Certificate reviewers should confirm the cerium and nitrogen windows rather than trusting a “253 MA” shop nickname or a TP309S-family PMI without Ce and N present. Product analysis, when ordered, applies A480 tolerances with Ce digits noted as UNCERTAIN above if the ordered A480 edition differs. EN 10204 3.1 is default; 3.2 when required. Dual SA-213/A213 names appear only when dual marking was ordered.

Packaging and Shipping

S30815 tube leaves SHH STEEL bundled, capped or end-protected, and tagged for export or domestic delivery according to length mix and bend form. Bundle tags repeat ASME SA-213 UNS S30815, heat number, size, and wall basis so receivers can match the 3.1 certificate — including Ce and N — without opening every bundle.

Export packing uses seaworthy bundling appropriate for pickled stainless. Marking follows SA-213 and any dual-mark text the PO adds, referencing A213 UNS S30815 only when dual ASTM marking was ordered. The commercial 253 MA nickname may appear in packing notes for routing, but the stencil and MTC still carry UNS S30815.

Why Choose SHH STEEL

SHH STEEL treats ASME SA213 UNS S30815 as a Code Book Ce–N high-temperature product with enforceable C 0.05–0.10%, Si 1.40–2.00%, Mn ≤0.80%, Cr 20–22%, Ni 10–12%, N 0.14–0.20%, Ce 0.03–0.08%, 87/45 ksi tensile, 40% elongation, hardness, and marking rules — not as “309S with a trademark sticker” checked only by a Cr PMI peak. Enquiry review verifies the cerium and nitrogen windows before release.

That stops silent substitution with TP309S or TP310S heats on datasheets that actually require S30815. We keep SA-213 and A213 independent, dual-mark only on request, and put Ce and N on the 3.1 certificate so inspectors can verify the grade. The commercial 253 MA nickname is allowed for routing — it never replaces S30815 on the MTC.

Cross-links: SA213 TP309S, SA213 UNS S30615, SA213 TP310S, hub SA213/SA213M.

Supply Capability

SHH STEEL can supply ASME SA213 UNS S30815 stainless steel tube against the edition and finish route named on your enquiry. The capability table below summarizes sizes, finishes, and documents we regularly quote, followed by the Stock / Available sizes map for Ce–N high-temperature furnace and heat-exchanger tube.

Item SHH STEEL capability for UNS S30815
Standard ASME SA213 / SA213M (dual A213 marking on request)
Grade UNS S30815 (no TP letter)
Product form Seamless only — cold-finished and hot-finished
Size Typical OD × min wall (or average wall) in the SA-213 usual band; other diameters by agreement
Wall / gauge Minimum wall or average wall; BWG / gauge callouts accepted on enquiry
Length Cut-to-length for furnace / HX bundles; U-bend by agreement
Documentation EN 10204 3.1 MTC with Ce / N windows; witness on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

Stock / Available sizes

SHH STEEL quotes S30815 against a stock-and-mill enquiry range rather than a frozen SKU or tonnage list. Representative OD × wall / BWG combinations below are an enquiry map for Ce–N high-temperature furnace and heat-exchanger tube — confirm live availability and cut lengths on the RFQ.

OD (in.) Typical wall / BWG enquiry band Notes
1/2 – 1 BWG 16–12 / ~0.065–0.109 in. Small HX / instrument sizes
1-1/4 – 2 BWG 14–10 / ~0.083–0.134 in. Common furnace / HX band
2-1/2 – 3 0.120 – 0.250 in. min wall Heavier HX / furnace wall
3-1/2 – 5 0.180 – 0.300 in. min wall Upper usual SA-213 OD by agreement

Send OD × wall (or BWG), wall basis, quantity, length mix, finish route, and any dual-mark needs with the RFQ so we can align mill capacity to the Ce/N package on the first reply.

FAQ

Is ASME SA-213 the same as ASTM A213 for UNS S30815?
No. ASME SA-213 / SA-213M is the ASME Code Book adoption; ASTM A213 / A213M is the separate ASTM product specification. Chemistry — including C 0.05–0.10%, Si 1.40–2.00%, Mn ≤0.80%, Cr 20.0–22.0%, Ni 10.0–12.0%, N 0.14–0.20%, and Ce 0.03–0.08% — tensile 87/45 ksi, elongation 40%, and hardness floors align in the shared grade text family, but the standards remain independent documents. Dual marking is a purchase-order option, not proof that the two titles are one standard.
Does ASME SA213 UNS S30815 have a TP grade letter?
No. S30815 appears in the stainless chemistry table without a TP letter (Footnote C practice). Order and mark by UNS S30815 under ASME SA-213 / SA-213M. Do not invent a “TP30815” stencil or assume the grade dual-stamps as TP309S or TP310S. The purchase order and MTC should carry the UNS designation explicitly so inspectors can match Ce, N, and tensile to the correct row.
Is 253 MA the same as ASME SA213 UNS S30815?
253 MA is a commercial / trademark shop name for the Ce–N chemistry family around S30815. It is useful for routing, but it does not replace ASME SA-213 UNS S30815 on the purchase order or the MTC. SHH STEEL will stencil and certify UNS S30815; packing notes may mention 253 MA only as a buyer routing aid when requested. Always confirm Ce 0.03–0.08% and N 0.14–0.20% against the certificate.
How does S30815 differ from TP309S under SA-213?
S30815 adds intentional silicon 1.40–2.00%, nitrogen 0.14–0.20%, and cerium 0.03–0.08%, with manganese capped at ≤0.80% and a 87/45 ksi tensile floor with 40% elongation. TP309S uses Si ≤1.00%, no mandatory Ce or N, Mn ≤2.00%, and a 75/30 ksi floor. Chromium bands overlap in the low-20s, but the Ce–N package and tensile set are not interchangeable. Do not accept a TP309S certificate as S30815 clearance.
What hardness limit applies to ASME SA213 UNS S30815 tube?
Table 4 caps S30815 hardness at 217 HBW or 95 HRB — higher than the 192 HBW / 90 HRB commodity austenitic ceiling. Hardness is checked together with the 87/45 ksi tensile set and 40% elongation. A hardness result alone does not prove Ce/N compliance; certificate reviewers should still read the cerium and nitrogen windows on the MTC.
What heat treatment applies to SA213 UNS S30815?
Solution treatment at a minimum of 1920 °F [1050 °C] followed by rapid cooling is the public path. That temperature sits slightly above the 1900 °F commodity austenitic minimum. There is no mandatory ASTM grain-size number for this grade in the public heat-treatment column. Footnote F / A262 attachment on the ordered edition is UNCERTAIN — confirm against the Code Book text named on the PO before assuming S4 test obligations.
Should I order minimum wall or average wall for S30815?
Furnace, boiler, and heat-exchanger datasheets that pick S30815 usually assume minimum wall. Average wall is acceptable when the purchase order says so and the general requirements for the ordered finish are applied. State wall basis, OD × wall or BWG, and length mix on the RFQ so the mill does not default to a basis your inspector will reject at receiving.
Is S30815 suitable for wet chloride heat-exchanger service?
Not as a default upgrade. S30815 is framed for high-temperature oxidation and scaling resistance with the Ce–N–Si package. Aggressive aqueous chlorides usually need molybdenum-bearing, duplex, or other project-specified alloys instead of a Ce–N high-temperature austenitic. Ask for a corrosion review before substituting S30815 into a wet-chloride HX datasheet that never named the UNS.
Does ASME SA213 UNS S30815 cover welded or HCW tube?
No. ASME SA-213 for this stainless series is a seamless boiler, superheater, and heat-exchanger tube product standard. SHH STEEL supplies S30815 as seamless cold-finished or hot-finished tube only. Welded (WLD) or heavily cold-worked welded (HCW) manufacturing types are outside this page’s product form and are not offered as a Manufacturing Types split under the SA213 UNS S30815 listing.
Can SHH STEEL dual-certify SA-213 and A213 for S30815?
Yes, when the purchase order asks for dual marking and the heat meets both product standards’ grade text for UNS S30815. Dual marking is a documentation and stencil option — it does not merge the two standards into one title. For non-Code purchases that only want the ASTM twin, see A213 UNS S30815; for Code-led work, keep SA-213 as the lead standard on the PO.
How does S30815 differ from high-Si Al UNS S30615 under SA-213?
S30815 is a Ce–N story (Ce 0.03–0.08%, N 0.14–0.20%, Si 1.40–2.00%) with an 87/45 ksi floor and 40% elongation. S30615 is a Si–Al story (Si 3.2–4.0%, Al 0.8–1.5%) with a 90/40 ksi floor and no mandatory cerium or nitrogen. They are related high-temperature concepts, not dual stamps. If the material list names aluminium or Si above 3%, review S30615; if it names cerium and nitrogen, review S30815.

Conclusion

ASME SA213 UNS S30815 is the Ce–N high-temperature seamless stainless steel tube grade for Code boiler, superheater, furnace, and heat-exchanger service when C 0.05–0.10%, Si 1.40–2.00%, Mn ≤0.80%, Cr 20.0–22.0%, Ni 10.0–12.0%, N 0.14–0.20%, Ce 0.03–0.08%, an 87/45 ksi tensile floor with 40% elongation, hardness max 217 HBW / 95 HRB, and a 1920 °F solution anneal are required together. SHH STEEL supplies cold-finished and hot-finished seamless tube in the usual OD × wall / BWG band with EN 10204 3.1 MTCs that report the Ce and N windows. The commercial 253 MA nickname does not replace UNS S30815 on the certificate. For quotations and technical review, contact admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *