ASME SA213 TP XM-15 Stainless Steel Tube | ASME SA213 Stainless Steel - SHH STEEL

ASME SA213 TP XM-15 Stainless Steel Tube

ASME SA213 XM-15 / UNS S38100 high-silicon high-nickel seamless boiler, superheater and heat-exchanger tube — C ≤0.08%, Si 1.50–2.50%, Cr 17.0–19.0%, Ni 17.5–18.5%, P/S ≤0.030%, no Mo/Nb/Ti requirement, Table 4 75/30 ksi with elongation 35% min, hardness max 192 HBW / 90 HRB, 1900 °F solution anneal (Footnote F). SHH STEEL supplies cold-finished and hot-finished seamless tube with EN 10204 3.1 MTCs that report the Si and Ni windows together. Commercial shop name 18-18-2 does not replace XM-15 on the MTC.
Grade
XM-15 / UNS S38100
Standard
ASME SA213 / SA213M
Product form
Seamless boiler / superheater / heat-exchanger tube (cold-finished and hot-finished)
Size
Typical OD × min wall (or average wall) within ~1/8 in. [3.2 mm] ID to 5 in. [127 mm] OD and ~0.015–0.500 in. [0.4–12.7 mm] wall; other diameters by agreement
Share:
Overview
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA213 TP XM-15 Stainless Steel Tube

ASME SA-213 / SA-213M is the ASME Boiler and Pressure Vessel Code Book adoption of the seamless ferritic and austenitic alloy-steel boiler, superheater, and heat-exchanger tube product text. When Code-stamped boilers, superheaters, or heat exchangers invoke that adoption by name, SA-213 is the governing product standard for this high-silicon, high-nickel austenitic tube — written as its own Code Book line, not as a merged synonym of ASTM A213. Begin from SA213/SA213M when the enquiry is Code-led.

Grade XM-15 / UNS S38100 is the high-Si / high-Ni austenitic row inside that stainless family. Melting carbon is capped at 0.08%, silicon sits in a deliberate 1.50–2.50% band, chromium at 17.0–19.0%, and nickel at 17.5–18.5% — roughly twice the nickel of classic TP304 — with phosphorus and sulfur each held to ≤0.030%. Molybdenum, nitrogen, niobium, and titanium have no requirement on this public row. Table 4 sets tensile at 75 ksi [515 MPa] / 30 ksi [205 MPa] with elongation 35% minimum and hardness max 192 HBW / 90 HRB. Buyers who write “18-18-2 HX tube” on a bill of materials still need to name SA-213 Grade XM-15 / UNS S38100 on the purchase order so the mill applies the tube product standard, minimum-wall rules, and the Si/Ni windows together. This is not a dual stamp of TP304, TP310S, or the higher-Si aluminium-bearing UNS S30615.

SHH STEEL can supply ASME SA213 TP XM-15 as seamless cold-finished and hot-finished tube in the usual OD × wall / BWG band, with EN 10204 3.1 certificates that report the silicon and nickel windows together with the 75/30 ksi tensile set, 35% elongation, and hardness. Dual SA-213/A213 marking is added only when the purchase order asks; the live twin is A213 TP XM-15.

Shop names include “XM-15,” “S38100,” and “18-18-2.” Helpful for routing; the commercial 18-18-2 nickname does not replace XM-15 on the MTC. The purchase order should still carry ASME SA-213 Grade XM-15 / UNS S38100, wall basis, OD × wall or BWG, finish route, and any Supplementary Requirements when needed. Sister SA213 pages include SA213 TP304, SA213 TP310S, SA213 TP XM-19, and SA213 UNS S30615 when that pack is live. Seamless only — no Manufacturing Types (SML / WLD / HCW) product-form split on this page.

Chemical Composition of SA213 XM-15

Two chemistry layers matter for XM-15 under ASME SA-213. Melting analysis is mandatory for every heat; product analysis on finished tube applies only when Supplementary Requirement wording or the purchase order invokes it through the general requirements (commonly ASTM A1016/A1016M), with tolerances typically from ASTM A480/A480M Table A1.1. The defining package for a reviewer is silicon 1.50–2.50% together with nickel 17.5–18.5% and chromium 17.0–19.0% — not a classic 18-8 nickel window and not a molybdenum addition. Phosphorus and sulfur are each capped at 0.030%, tighter than the 0.045% / 0.030% pair on many sister austenitics. Carbon ≤0.08% matches the non-L 18-8 ceiling; there is no mandatory Nb, Ti, Mo, or N band on the public row.

The tables below reproduce the melt limits for XM-15 / UNS S38100, the product-analysis limits from A480 Table A1.1 practice, and a short Si/Ni snapshot against TP304 and related high-Si grades. Later SA-213 / A213 editions place austenitic stainless grades in Table 2 (older editions used Table 1); confirm the ordered edition on the purchase order.

Melting analysis (heat / ladle analysis)

Element XM-15 (UNS S38100) melting analysis
Carbon (C) ≤ 0.08
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.030
Sulfur (S) ≤ 0.030
Silicon (Si) 1.50 – 2.50
Chromium (Cr) 17.0 – 19.0
Nickel (Ni) 17.5 – 18.5
Molybdenum (Mo) … (no requirement)
Nitrogen (N) … (no requirement)
Niobium (Nb) … (no requirement)
Titanium (Ti) … (no requirement)

Source: public SA-213 / A213 stainless chemistry table for Grade XM-15 / UNS S38100 (same grade text family). Confirm the ordered edition. Where ellipses appear, the ordered edition sets no requirement for that element. UNCERTAIN: exact edition year and stainless chem table number on the ordered Code Book text.

Product analysis — A480/A480M Table A1.1 tolerances applied

Element Melting Tolerance (A480 A1.1) Product analysis limit
Carbon (C) ≤ 0.08 0.01 over ≤ 0.09
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.030 0.005 over ≤ 0.035
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) 1.50 – 2.50 0.05 under / over 1.45 – 2.55
Chromium (Cr) 17.0 – 19.0 0.20 under / over 16.80 – 19.20
Nickel (Ni) 17.5 – 18.5 0.15 under / over 17.35 – 18.65

Product analysis is not automatic — order it when the project needs finished-tube chemistry, especially the silicon and nickel windows. UNCERTAIN: A480 product-tolerance digits for the Si 1.50–2.50 band should be confirmed against the ordered A480 edition if the PO makes product analysis contractual.

Si / Ni snapshot — TP304 / XM-15 / related high-Si grades

Element TP304 (S30400) XM-15 (S38100) Notes on related high-Si grades
Si ≤ 1.00 1.50 – 2.50 S30615 carries Si 3.2–4.0 plus Al 0.8–1.5 — not XM-15
Ni 8.0 – 11.0 17.5 – 18.5 Roughly double classic 18-8 nickel
Cr 18.0 – 20.0 17.0 – 19.0 Similar chromium band, different Si/Ni story
Mo / Al / Ce none required none required S30815 adds Ce–N; S30615 adds Al — separate UNS rows

Reading tip: a heat that clears TP304 still fails XM-15 if silicon sits at ≤1.00% or nickel sits near 8–11%. Do not accept a verbal “18-18-2” shop note as proof that the MTC prints XM-15 / S38100 with the Si and Ni windows satisfied.

Mechanical Properties of SA213 XM-15

Table 4 of the public SA-213 / A213 grade text family sets XM-15 tensile strength at 75 ksi [515 MPa] minimum and yield (0.2% offset) at 30 ksi [205 MPa] minimum — the same floors as TP304 and many sister austenitics. Elongation in 2 in. or 50 mm is 35% minimum, and hardness is capped at 192 HBW / 200 HV or 90 HRB. The high-Si / high-Ni chemistry does not raise the tensile floor; it changes which heat clears the grade stamp for oxidation-leaning or high-silicon purchase specifications that name S38100.

Property XM-15 requirement (Table 4)
Tensile strength, min 75 ksi [515 MPa]
Yield strength (0.2% offset), min 30 ksi [205 MPa]
Elongation in 2 in. or 50 mm, min 35%
Hardness, max 192 HBW / 200 HV or 90 HRB
Grain size No mandatory ASTM grain-size number

XM-15 has no mandatory ASTM grain-size number in the heat-treatment column. If a project datasheet asks for an E112 grain-size report, put that supplementary requirement on the purchase order rather than assuming base SA-213 includes it. Flattening and flaring follow the general requirements for the ordered size; hydrostatic or nondestructive examination follows the path selected on the PO.

Dimensions and Tolerances

Dimensional supply for ASME SA213 TP XM-15 is tube language — outside diameter × wall thickness (minimum wall or average wall) and, commercially, BWG / gauge — not ASME B36.19 pipe schedules as the primary size story. Usual SA-213 sizes run from about 1/8 in. [3.2 mm] inside diameter to 5 in. [127 mm] outside diameter, with minimum wall from about 0.015 to 0.500 in. [0.4 to 12.7 mm]; other diameters may be furnished when all other requirements are met.

Furnace, boiler, and heat-exchanger datasheets that pick high-Si XM-15 usually assume minimum wall — state wall basis on the purchase order. Outside-diameter and wall variations follow the general requirements invoked by SA-213 (commonly ASTM A1016/A1016M). The Si/Ni package does not change the dimensional tolerance tables; it changes which heat clears the grade stamp.

Item Typical SA213 XM-15 dimensional practice
Product form Seamless only (cold-finished or hot-finished)
Usual size band ~1/8 in. [3.2 mm] ID to 5 in. [127 mm] OD; wall ~0.015–0.500 in. [0.4–12.7 mm]
Wall basis Minimum wall (common for furnace / HX datasheets) or average wall if PO says so
OD / wall tolerance Per general requirements (commonly A1016/A1016M) for the ordered finish
Length Straight random / cut-to-length; U-bend by agreement

BWG / gauge callouts are accepted on enquiry; certificates should still show OD and wall in inch or millimetre units. U-bends and polished ID finishes are commercial options — they do not replace the silicon and nickel window checks.

Equivalent Grades

Equivalence talk for XM-15 should start from the Code Book product standard and the UNS, not from the commercial 18-18-2 nickname. ASME SA-213 Grade XM-15 / UNS S38100 is the governing designation on this page. ASTM A213 XM-15 is the separate ASTM twin used when dual marking or a non-Code purchase is agreed — it is not a substitute lead standard for an SA-213 order. Related high-Si or high-Ni grades (S30615, S30815, TP310S, XM-19) are sister options under the same hub family, not automatic dual stamps.

Designation Notes
ASME SA-213 / SA-213M Grade XM-15 Governing Code Book seamless boiler / HX tube product standard for this article
UNS S38100 Unified number in the stainless chemistry table
18-18-2 (commercial) Shop name for the high-Si / high-Ni chemistry family — does not replace XM-15 on the MTC
ASTM A213 XM-15 Separate ASTM product specification — dual-mark only when the PO asks; twin page A213 TP XM-15
Related high-Si Al grade UNS S30615 — Si 3.2–4.0 plus Al 0.8–1.5; not interchangeable with XM-15
Related Ce–N grade UNS S30815 — Ce 0.03–0.08, N 0.14–0.20; separate chemistry story
Related plate A240 / SA240 flat product in the same UNS family — order plate and tube under their own standards

Hub entry point: SA213/SA213M. When a bill of materials only says “18-18-2,” ask whether Si 1.50–2.50% and Ni 17.5–18.5% are actually required before shipping XM-15 or a TP304 / TP310S alternative.

Heat Treatment and Delivery Condition

XM-15 under ASME SA-213 is furnished solution treated at a minimum of 1900 °F [1040 °C], then quenched in water or cooled rapidly by other means. The heat-treatment table carries Footnote F for this grade: quench rate must be sufficient to prevent carbide re-precipitation, as demonstrable by the capability of tubes — heat treated by separate solution annealing or by direct quenching — to pass Practices A262, Practice E. The manufacturer is not required to run the A262 test unless the purchase order specifies it (see Supplementary Requirement S4).

Cold-finished versus hot-finished is a process and dimensional route, not a substitute for the anneal. Delivery condition for SHH STEEL XM-15 is solution annealed and pickled (or bright annealed by agreement), with anneal temperature and quench method on the EN 10204 3.1 certificate. Straightening, cutting, and end finishing follow heat treatment. XM-15 has no mandatory ASTM grain-size number in the heat-treatment column. If a project datasheet asks for an E112 grain-size report, put that supplementary requirement on the purchase order rather than assuming base SA-213 includes it.

Do not treat a verbal “annealed 18-18-2” note as proof that the mill ran the 1900 °F SA-213 path with Footnote F quench capability. UNCERTAIN: full Footnote F / S4 wording on the ordered edition — confirm against the Code Book text named on the PO.

Corrosion Resistance

XM-15 under ASME SA-213 is selected primarily for high-temperature oxidation and scaling resistance associated with elevated silicon and a high nickel window — furnace and process-heater framing — not as a general wet-chloride upgrade over TP304. The Si 1.50–2.50% band supports oxide-scale adherence relative to low-silicon 18-8 in many dry or mildly oxidizing services, but the grade is not a duplex or molybdenum-bearing superaustenitic for aggressive aqueous chlorides.

Where a datasheet mixes “18-18-2” with wet process condensates or chloride deposits, ask whether the service is actually looking for a molybdenum-bearing or duplex tube instead of a high-Si austenitic. SHH STEEL will not treat a silicon PMI peak alone as proof of aqueous corrosion suitability — chemistry, heat treatment, and the intended medium have to be read together.

Applications of SA213 XM-15 Tube

Typical ASME SA213 TP XM-15 placements are Code-stamped boiler, superheater, and heat-exchanger or furnace tubes where the material list names S38100 or explicitly requires Si 1.50–2.50% with Ni 17.5–18.5% — not generic “304 family” or “310” replacements. Process heaters and high-temperature HX bundles that already distinguish 18-18-2 chemistry from TP304 are the natural fit.

When the enquiry only says “18-18-2” without UNS language, confirm whether the buyer actually needs SA213 TP304, SA213 TP310S, or a higher-Si aluminium-bearing grade before substituting. SHH STEEL quotes XM-15 when the enquiry names the UNS or the Si/Ni package explicitly.

Weldability

XM-15 welds as a high-silicon, high-nickel austenitic. Filler selection should respect the elevated silicon and the ~18% nickel window rather than copying a plain ER308 procedure without review. Matching or near-matching austenitic fillers with adequate silicon and nickel are the usual starting point; confirm chemistry against the WPS when the project treats Si/Ni as contractual on the weld metal as well as the tube.

Autogenous welds and thin-wall HX joints need heat-input control to protect the as-annealed condition near the HAZ. Post-weld heat treatment is not a default SA-213 requirement for this grade — if the vessel code or the buyer wants a separate resolution anneal after welding, write that as a negotiated step. SHH STEEL can coordinate weld coupons when the PO asks.

Surface Finishes

Standard mill delivery for ASME SA213 TP XM-15 is solution annealed and pickled, leaving a clean matte finish suitable for furnace, boiler, and heat-exchanger tube duty. Bright annealing is available by agreement when OD appearance or polish steps favor it.

ID/OD polish and U-bend conditioning are commercial additions — they do not replace the silicon and nickel window checks. End caps and dry export packaging matter more than paint on pickled stainless.

SHH STEEL notes the ordered surface route on the packing list and aligns it with the MTC finish description for receiving inspection.

Inspection and Testing

Base ASME SA-213 testing for XM-15 includes heat analysis (C ≤0.08%, Si 1.50–2.50%, Cr 17.0–19.0%, Ni 17.5–18.5%, P/S ≤0.030%), tension tests to the 75/30 ksi floors with 35% elongation, hardness to 192 HBW / 90 HRB, and flattening / flaring tests for the ordered size. Hydrostatic testing or NDE follows the path selected on the purchase order.

Certificate reviewers should confirm the silicon and nickel windows rather than trusting an “18-18-2” shop nickname or a TP304-family PMI without Si ≥1.50%. Product analysis, when ordered, applies A480 tolerances with Si digits noted as UNCERTAIN above if the ordered A480 edition differs. A262 Practice E applies only when S4 is named on the PO. EN 10204 3.1 is default; 3.2 when required. Dual SA-213/A213 names appear only when dual marking was ordered.

Packaging and Shipping

XM-15 tube leaves SHH STEEL bundled, capped or end-protected, and tagged for export or domestic delivery according to length mix and bend form. Bundle tags repeat ASME SA-213 Grade XM-15, UNS S38100, heat number, size, and wall basis so receivers can match the 3.1 certificate — including Si and Ni — without opening every bundle.

Export packing uses seaworthy bundling appropriate for pickled stainless. Marking follows SA-213 and any dual-mark text the PO adds, referencing A213 TP XM-15 only when dual ASTM marking was ordered. The commercial 18-18-2 nickname may appear in packing notes for routing, but the stencil and MTC still carry XM-15 / S38100.

Why Choose SHH STEEL

SHH STEEL treats ASME SA213 TP XM-15 as a Code Book high-silicon high-nickel product with enforceable C ≤0.08%, Si 1.50–2.50%, Cr 17–19%, Ni 17.5–18.5%, P/S ≤0.030%, 75/30 ksi tensile, 35% elongation, hardness, and marking rules — not as “304 with extra silicon” checked only by a Si PMI peak. Enquiry review verifies the silicon and nickel windows before release.

That stops silent substitution with TP304 or TP310S heats on datasheets that actually require S38100. We keep SA-213 and A213 independent, dual-mark only on request, and put Si and Ni on the 3.1 certificate so inspectors can verify the grade. The commercial 18-18-2 nickname is allowed for routing — it never replaces XM-15 on the MTC.

Cross-links: SA213 TP304, SA213 TP310S, SA213 TP XM-19, hub SA213/SA213M.

Supply Capability

SHH STEEL can supply ASME SA213 TP XM-15 stainless steel tube against the edition and finish route named on your enquiry. The capability table below summarizes sizes, finishes, and documents we regularly quote, followed by the Stock / Available sizes map for high-Si / high-Ni furnace and heat-exchanger tube.

Item SHH STEEL capability for XM-15
Standard ASME SA213 / SA213M (dual A213 marking on request)
Grade XM-15 / UNS S38100
Product form Seamless only — cold-finished and hot-finished
Size Typical OD × min wall (or average wall) in the SA-213 usual band; other diameters by agreement
Wall / gauge Minimum wall or average wall; BWG / gauge callouts accepted on enquiry
Length Cut-to-length for furnace / HX bundles; U-bend by agreement
Documentation EN 10204 3.1 MTC with Si / Ni windows; S4 A262 / witness on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

Stock / Available sizes

SHH STEEL quotes XM-15 against a stock-and-mill enquiry range rather than a frozen SKU or tonnage list. Representative OD × wall / BWG combinations below are an enquiry map for high-Si / high-Ni furnace and heat-exchanger tube — confirm live availability and cut lengths on the RFQ.

OD (in.) Typical wall / BWG enquiry band Notes
1/2 – 1 BWG 16–12 / ~0.065–0.109 in. Small HX / instrument sizes
1-1/4 – 2 BWG 14–10 / ~0.083–0.134 in. Common furnace / HX band
2-1/2 – 3 0.120 – 0.250 in. min wall Heavier HX / furnace wall
3-1/2 – 5 0.180 – 0.300 in. min wall Upper usual SA-213 OD by agreement

Send OD × wall (or BWG), wall basis, quantity, length mix, finish route, and any dual-mark or A262 needs with the RFQ so we can align mill capacity to the Si/Ni package on the first reply.

FAQ

Is ASME SA-213 the same as ASTM A213 for XM-15?
No. ASME SA-213 / SA-213M is the ASME Code Book adoption; ASTM A213 / A213M is the separate ASTM product specification. Chemistry — including C ≤0.08%, Si 1.50–2.50%, Cr 17.0–19.0%, Ni 17.5–18.5%, and P/S ≤0.030% — tensile 75/30 ksi, elongation 35%, and hardness floors align in the shared grade text family, but the standards remain independent documents. Dual marking is a purchase-order option, not proof that the two titles are one standard.
Does SA213 TP XM-15 cover welded or HCW tube?
No. ASME SA-213 for this stainless series is a seamless boiler, superheater, and heat-exchanger tube product standard. SHH STEEL supplies XM-15 as seamless cold-finished or hot-finished tube only. Welded (WLD) or heavily cold-worked welded (HCW) manufacturing types are outside this page’s product form and are not offered as a Manufacturing Types split under the SA213 TP XM-15 listing.
What chemistry defines ASME SA213 XM-15 versus TP304?
XM-15 / UNS S38100 requires silicon 1.50–2.50% and nickel 17.5–18.5% with chromium 17.0–19.0% and P/S ≤0.030%. Classic TP304 uses Si ≤1.00% and Ni 8.0–11.0% with Cr 18–20%. A heat that clears TP304 still fails XM-15 if silicon sits at the low-Si ceiling or nickel sits near the 18-8 window. Do not accept a “304 with extra silicon” verbal note as S38100 compliance.
Is 18-18-2 the same as ASME SA213 XM-15?
18-18-2 is a commercial shop name for the high-Si / high-Ni chemistry family around S38100. It is useful for routing, but it does not replace ASME SA-213 Grade XM-15 / UNS S38100 on the purchase order or the MTC. SHH STEEL will stencil and certify XM-15 / S38100; packing notes may mention 18-18-2 only as a buyer routing aid when requested.
How does XM-15 differ from high-Si UNS S30615 under SA-213?
S30615 carries a much higher silicon band (about 3.2–4.0%) plus aluminium 0.8–1.5% — a different oxidation-alloy story from XM-15’s Si 1.50–2.50% / Ni 17.5–18.5% package without mandatory aluminium. They are related high-Si concepts, not dual stamps. If the material list names aluminium or Si above 3%, review S30615 instead of assuming XM-15 covers it.
What hardness limit applies to ASME SA213 XM-15 tube?
Table 4 caps XM-15 hardness at 192 HBW / 200 HV or 90 HRB — the same ceiling as TP304. Hardness is checked together with the 75/30 ksi tensile set and 35% elongation. A hardness result alone does not prove Si/Ni compliance; certificate reviewers should still read the silicon and nickel windows on the MTC.
What heat treatment applies to SA213 XM-15?
Solution treatment at a minimum of 1900 °F [1040 °C] followed by rapid cooling is the public path, with Footnote F quench-capability language tied to A262 Practice E demonstrability when that test is ordered. The manufacturer is not required to run A262 unless Supplementary Requirement S4 is on the purchase order. There is no mandatory ASTM grain-size number for this grade in the public heat-treatment column.
Should I order minimum wall or average wall for XM-15?
Furnace, boiler, and heat-exchanger datasheets that pick XM-15 usually assume minimum wall. Average wall is acceptable when the purchase order says so and the general requirements for the ordered finish are applied. State wall basis, OD × wall or BWG, and length mix on the RFQ so the mill does not default to a basis your inspector will reject.
Is XM-15 suitable for wet chloride heat-exchanger service?
Not as a default upgrade. XM-15 is framed for high-temperature oxidation and scaling resistance with elevated silicon and high nickel. Aggressive aqueous chlorides usually need molybdenum-bearing, duplex, or other project-specified alloys instead of a high-Si austenitic. Ask for a corrosion review before substituting XM-15 into a wet-chloride HX datasheet that never named S38100.
Can SHH STEEL dual-certify SA-213 and A213 for XM-15?
Yes, when the purchase order asks for dual marking and the heat meets both product standards’ grade text for XM-15 / UNS S38100. Dual marking is a documentation and stencil option — it does not merge the two standards into one title. For non-Code purchases that only want the ASTM twin, see A213 TP XM-15; for Code-led work, keep SA-213 as the lead standard on the PO.
Does XM-15 require niobium or titanium stabilization?
No. The public SA-213 / A213 chemistry row for XM-15 / S38100 sets no requirement for niobium or titanium. Stabilization is not the grade’s defining story — the silicon and nickel windows are. If a datasheet asks for Nb- or Ti-stabilized tube, it is probably looking for TP347, TP321, or another row, not XM-15.

Conclusion

ASME SA213 TP XM-15 / UNS S38100 is the high-silicon high-nickel seamless stainless steel tube grade for Code boiler, superheater, furnace, and heat-exchanger service when C ≤0.08%, Si 1.50–2.50%, Cr 17.0–19.0%, Ni 17.5–18.5%, P/S ≤0.030%, a 75/30 ksi tensile floor with 35% elongation, hardness max 192 HBW / 90 HRB, and a 1900 °F solution anneal with Footnote F are required together. SHH STEEL supplies cold-finished and hot-finished seamless tube in the usual OD × wall / BWG band with EN 10204 3.1 MTCs that report the Si and Ni windows. The commercial 18-18-2 nickname does not replace XM-15 on the certificate. For quotations and technical review, contact admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X