Q390GJD building steel plates GB/T 19879 under gantry cranes at SHH STEEL yard

GB/T 19879 Q390GJD Building Steel Plate Supplier

GB/T 19879 Q390GJD is high-performance building structure steel plate with 390 MPa minimum yield, a 390 – 510 MPa yield window, yield ratio ≤0.83 and 47 J Charpy impact at −20°C. SHH STEEL supplies Q390GJD mill-direct, 6 mm – 150 mm, with Z15, Z25 or Z35 options and full heat and product analysis.
Keywords
Q390GJD, Q390GJD steel plate, GB/T 19879 Q390GJD, Q390GJ-D, Q390GJDZ15, Q390GJDZ25, Q390GJDZ35, Q390GJ, building structure steel plate, Q390GJD supplier
Equivalent Grades
GB/T 19879 Q390GJD / GB/T 1591 Q390ND or Q390MD (no yield cap) / EN 10025 S420 (next step up; no S390) / ASTM A572 Gr.55 (380 MPa) / JIS G3106 SM520 — Material Specification: GB/T 19879-2023 (supersedes GB/T 19879-2015) — Delivery: CR, NR, N, NT, TMCP or TMCP+T; −20°C impact
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q390GJD vs Q390D
Q390GJ vs Q355GJ
Material Comparison
Z15 / Z25 / Z35
Equivalent Material Grades
Weldability
Heat Treatment and Delivery Condition
Dimensions
Tolerances
Supplementary Requirements
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 19879 Q390GJD Building Steel Plate?

Q390GJD, also written Q390GJ-D or Q390 GJD, is hot-rolled steel plate for building structures under GB/T 19879. Q means yield, 390 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and D is the quality grade: Charpy V-notch at −20°C, at least 47 J.

The GJ rules are what the structural engineer is paying for. Q390GJD sets a maximum yield as well as a minimum, caps the yield ratio, limits carbon equivalent by thickness and delivery route, and keeps P and S low. The frame then yields where the designer expects.

Q390GJD is the 390 MPa plate for −20°C details: thick column splices, brace nodes and base plates in cold regions. At this strength the D letter matters more than at 235 MPa, because thicker, stronger plate has less toughness margin in the heat-affected zone.

GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. The yield-ratio cap for Q390GJ is 0.83 in both editions. What changed is the thickness effect: the 2015 edition stepped yield down 10 MPa above 50 mm, while the 2023 edition holds 390–510 MPa (ReH) from 16 mm to 100 mm. Delivery codes now read CR/NR/N/NT and TMCP/TMCP+T. Sister grades are listed under GB/T 19879, including Q390GJB.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q390GJD cut to size with an EN 10204 3.1 or 3.2 certificate.

Material Specification

Specification element Requirement SHH STEEL compliance
Plate standard GB/T 19879-2023 Q390GJD (GB/T 19879-2015 when the drawing names it) Confirmed
Thickness for Q390GJ 6 mm – 150 mm Confirmed
Yield strength 390 MPa min; 390 – 510 MPa for 16–100 mm Confirmed
Tensile strength 510 – 660 MPa (to 100 mm) Confirmed
Yield ratio ≤ 0.83 Printed on MTC
Quality grade D, Charpy V at −20°C, KV2 ≥ 47 J, longitudinal Confirmed
Delivery condition CR, NR, N, NT, TMCP or TMCP+T As ordered
Through-thickness Z15, Z25 or Z35 to GB/T 5313 As ordered
Dimensions GB/T 709-2019, thickness tolerance Class B Confirmed
Chemistry report Heat analysis + CEV; product analysis on request Confirmed
Certificate EN 10204 3.1 or 3.2 As ordered

Grades often confused with it are GB/T 1591 Q390ND and ASTM A572 Gr.55. None of them carries the GJ yield cap or yield-ratio rule.

Chemical Composition: Heat Analysis and Product Analysis

GB/T 19879 controls chemistry twice. The heat (ladle) analysis is taken from the melt and must meet Table 1 of the standard. The product analysis is taken from the finished plate and may sit slightly outside Table 1, by the permitted deviations of GB/T 222 (clause 7.1.4). Both are valid acceptance checks, but they are not the same number.

Table 1 below is the heat analysis for Q390GJD. The columns on the right show the quality-grade groups at Q390GJ.

Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %

Element Q390GJD heat analysis (%) Q390GJ B / C Q390GJ D / E
C, max 0.18 0.20 0.18
Si, max 0.55 0.55 0.55
Mn, max 1.70 1.70 1.70
P, max 0.020 0.025 0.020
S, max 0.010 0.015 0.010
V, max 0.200 0.200 0.200
Nb, max 0.070 0.070 0.070
Ti, max 0.030 0.030 0.030
Als, min 0.015 0.015 0.015
Cr, max 0.30 0.30 0.30
Cu, max 0.30 0.30 0.30
Ni, max 0.70 0.70 0.70
Mo, max 0.50 0.50 0.50
V + Nb + Ti, max (if combined) 0.22 0.22 0.22

Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. V + Nb + Ti, when combined, is limited to 0.22%. These limits are the same in the 2015 and 2023 editions.

B and C grades share one chemistry column. D and E grades tighten carbon to 0.18%, phosphorus to 0.020% and sulfur to 0.010%, because they are tested at −20°C and −40°C.

Table 2. Product analysis limits for Q390GJD, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %

Element Heat limit (%) Permitted deviation, GB/T 222-2025 Table 1 Q390GJD product analysis limit (%)
C ≤ 0.18 +0.02 ≤ 0.20
Si ≤ 0.55 +0.05 ≤ 0.60
Mn ≤ 1.70 +0.06 ≤ 1.76
P ≤ 0.020 +0.005 ≤ 0.025
S ≤ 0.010 +0.005 ≤ 0.015
V ≤ 0.200 +0.02 ≤ 0.220
Nb ≤ 0.070 ±0.005 ≤ 0.075 (Table 1 lists Nb to 0.060%; agree above that)
Ti ≤ 0.030 +0.02 ≤ 0.050
Als ≥ 0.015 −0.003 ≥ 0.012
Cr ≤ 0.30 +0.05 ≤ 0.35
Cu ≤ 0.30 +0.05 ≤ 0.35
Ni ≤ 0.70 +0.05 ≤ 0.75
Mo ≤ 0.50 Not listed in Table 1 Agree in contract (alloy-steel Table 2 would give ≤ 0.52)

How to read Table 2. The band is chosen by the Table 1 upper limit. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn ≤1.70% falls in the 0.80–1.70% band, so +0.06%. For one heat an element may deviate in one direction only.

GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).

Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.

Mechanical Properties

Values below follow Table 3 and Table 5 of GB/T 19879-2023 for Q390GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.

Thickness Upper yield ReH (MPa) Tensile Rm (MPa) Yield ratio, max Elongation A, min
6 – 16 mm ≥ 390 510 – 660 0.83 20%
> 16 – 100 mm 390 – 510 510 – 660 0.83 20%
> 100 – 150 mm 370 – 490 490 – 640 0.83 20%

The 2015 edition used lower yield ReL and stepped yield down 10 MPa above 50 mm. Write the edition on the order so the mill tests to the right table.

Test Q390GJD requirement
Charpy V-notch, longitudinal −20°C, KV2 ≥ 47 J, average of 3
Single value One value may fall below the average requirement, not below 70% of it (GB/T 17505)
Sub-size specimens 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy
180° bend Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2)
Through-thickness (≥ 15 mm) Z15, Z25 or Z35 to GB/T 5313, when ordered

Density for theoretical weight is 7.85 g/cm³.

Q390GJD vs Q390D (GB/T 1591): Same 390 MPa, Different Job

Q390 under GB/T 1591 and Q390GJD share a number and little else. Q390 steps yield down as plate gets thicker: by 40–63 mm the minimum is 360 MPa. Q390GJD holds 390 MPa to 100 mm, then caps it at 510 MPa.

That matters most in thick column plate, which is exactly where 390 MPa gets specified. A 60 mm flange in GB/T 1591 Q390 is really a 360 MPa flange.

Property Q390D (GB/T 1591-2018) Q390GJD (GB/T 19879-2023)
Yield at 16 mm 390 MPa 390 MPa
Yield at 16–40 mm 380 MPa min 390 – 510 MPa
Yield at 40–63 mm 360 MPa min 390 – 510 MPa
Yield upper limit None 510 MPa to 100 mm
Yield ratio No limit ≤ 0.83
Tensile to 100 mm 490 – 650 MPa 510 – 660 MPa
Impact −20°C, 34 J −20°C, 47 J
C / P / S, max Per GB/T 1591 grade 0.18 / 0.020 / 0.010%
Ni, max Per GB/T 1591 grade 0.70%
CEV ≤ 50 mm Per GB/T 1591 route 0.45% (CR/N), 0.40% (TMCP)

The normalized and TMCP equivalents at −20°C are GB/T 1591 Q390ND and GB/T 1591 Q390MD. Both improve toughness; neither adds the GJ yield cap.

Q390GJD vs Q355GJD: When to Step Up a Strength Level

Check Q355GJD Q390GJD
Yield, 16–100 mm 355 – 475 MPa 390 – 510 MPa
Tensile, to 100 mm 490 – 610 MPa 510 – 660 MPa
Yield ratio ≤ 0.83 ≤ 0.83
CEV ≤ 50 mm 0.43% (AR/N) 0.45% (CR/N)
CEV TMCP ≤ 50 mm 0.38% 0.40%
Max thickness 200 mm 150 mm
Ni / Mo, max 0.30 / 0.20% 0.70 / 0.50%

The yield gain is 35 MPa, about 10%. In a strength-governed column that is roughly a 9% cut in plate thickness and weld volume. CEV rises only 0.02 points on CR/N plate.

Above 150 mm Q390GJ is not available, so very heavy sections stay at Q355GJ. Below that, compare tonnage, weld time and plate price, not plate price alone. See Q345GJD for the 355 MPa plate.

Q390GJB, Q390GJC, Q390GJD or Q390GJE: Which Quality Grade?

Grade Impact temperature Energy, min C / P / S max (%) Typical use
Q390GJB +20°C 47 J 0.20 / 0.025 / 0.015 Heated interiors, mild climates
Q390GJC 0°C 47 J 0.20 / 0.025 / 0.015 Cold regions, exposed frames
Q390GJD −20°C 47 J 0.18 / 0.020 / 0.010 Severe winters, thick welded nodes
Q390GJE −40°C 47 J 0.18 / 0.020 / 0.010 Arctic and low-temperature sites

Strength, yield ratio and CEV do not change from B to E. Only the impact temperature and the D/E chemistry move. Pick the letter from the lowest service or erection temperature.

Q390GJD is the letter for −20°C design temperatures, and the one we suggest when the plate is thick and restrained. For the same letter at another strength level: one level up, Q420GJD; one level down, Q345GJD.

Q390GJDZ15, Q390GJDZ25 and Q390GJDZ35: Through-Thickness Plate

Thick plate loaded across its thickness can tear in layers under weld shrinkage. Column flanges at beam-flange welds, diaphragm plates in box columns and base plates under heavy tension are the usual places. A Z grade guarantees ductility in that direction.

The designation adds the Z level to the grade, for example Q390GJDZ25. Z tests apply to plate 15 mm and thicker and follow GB/T 5313-2023.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

The D melt already caps S at 0.010%, the Z15 limit, so Z25 and Z35 are the levels that change the steelmaking.

GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.

Ask for Z only where the joint needs it. Over-specifying Z35 across a whole order adds cost and lead time without helping the frame.

Equivalent Material Grades

EN 10025 has no 390 MPa grade, so European reviewers usually check Q390GJ against S420 and accept it on the yield floor, or against S355 with a strength upgrade. Neither has the GJ ratio cap.

Designation Region Standard Notes
Q390GJD China GB/T 19879-2023 Grade on this page
GB/T 1591 Q390ND China GB/T 1591-2018 Normalized; no yield cap
GB/T 1591 Q390MD China GB/T 1591-2018 TMCP; no yield cap
EN 10025-4 S420M Europe EN 10025-3/-4 Next step up (no S390 in EN); strength only
EN 10025-2 S355K2 Europe EN 10025-2 Next step down
ASTM A572 Gr.55 USA ASTM A572 380 MPa; one step lower
JIS G3106 SM520C Japan JIS G3106 355 MPa class; no ratio rule

For mill-direct supply under the GB family, the normalized and TMCP Q390 grades in GB/T 1591 are the nearest relatives.

Weldability

GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q390GJD certificate:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Delivery condition CEV ≤ 50 mm CEV > 50 – 100 mm CEV > 100 – 150 mm Pcm ≤ 50 mm Pcm > 50 – 100 mm Pcm > 100 – 150 mm
CR, NR, N, NT 0.45 0.47 0.49 0.28 0.30 0.31
TMCP, TMCP+T 0.40 0.43 By agreement 0.26 0.27 —

CR/N Q390GJ sits at 0.45% CEV to 50 mm, TMCP plate at 0.40%. The TMCP route is the easier one to weld thick, and we suggest it for column plate above 60 mm.

The D letter helps: carbon is capped at 0.18% and P and S are lower, which reduces hot-cracking and HAZ embrittlement risk.

Typical consumables: E50- or E55-class low-hydrogen electrodes (E5515 types) or matching ER55 wire. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.

Heat Treatment and Delivery Condition

Q390GJD may be delivered CR, NR, N or NT, or TMCP / TMCP+T. QT is not listed for Q390GJ in Table 2. Each route has its own CEV and Pcm limits, so the route is part of the specification, not a mill detail.

TMCP gives the lowest CEV and the best weldability. N or NT gives the most uniform through-thickness properties on heavy plate. QT holds strength in the thickest sizes.

Agree the route before price. A mill quoting N where the drawing assumed TMCP CEV is not quoting the same plate. TMCP references: GB/T 1591 Q390MD; normalized: GB/T 1591 Q390ND.

Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.

Dimensions

Usual Q390GJD supply range from SHH STEEL:

  • Thickness: 6 mm – 150 mm; most orders 8 mm – 100 mm
  • Width: 1500 mm – 3000 mm standard; wider by mill confirmation
  • Length: 3000 mm – 12000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³

Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.

Tolerances

GB/T 19879-2023 sends dimensions and shape to GB/T 709-2019. Thickness tolerance is Class B by default: fixed minus 0.30 mm, plus by thickness and width. Class C (zero minus) is available by agreement.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.

Supplementary Requirements

Q390GJD already fixes strength, yield ratio, CEV and −20°C impact. Anything more goes on the purchase order.

  • Edition: GB/T 19879-2023 or -2015. Never write only Q390.
  • Product analysis: ask for a second chemistry column checked to GB/T 222.
  • Through-thickness: add Z15, Z25 or Z35, e.g. Q390GJDZ25.
  • Delivery condition: name it (CR, NR, N, NT, TMCP or TMCP+T) if the welding procedure depends on it.
  • Ultrasonic testing beyond Z plates: GB/T 2970 class, or EN 10160 / ASTM A578.
  • Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the D letter.
  • Tolerance: Class C for zero minus.
  • Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.

Q390GJD Price Factors and How to Order

A Q390GJD price per ton is a base price plus extras. The extras explain most gaps between quotes.

Cost driver Effect on price
GJ grade over general Q390 plate Grade extra for cleaner steel, yield control and CEV
Quality letter D Extra for −20°C testing and the cleaner D melt
Delivery route TMCP or N; NT adds furnace time
Thickness Thin and very thick plate carry size extras; 10–60 mm is usually cheapest
Z15 / Z25 / Z35 Desulfurization, plate-by-plate Z test and UT; Z35 costs most
Width and length Over 3000 mm wide or 12 m long needs mill confirmation
Quantity per size Mill rolling minimums per size; small lots come from stock or combined rolling
Inspection and cutting 3.2 witness, profile cutting, blasting and priming are quoted per item

To get a firm quote in one round, send:

  • Grade and edition, e.g. Q390GJDZ25 to GB/T 19879-2023
  • Thickness × width × length and pieces or tonnes
  • Delivery route, UT standard and class
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q390GJE.

Applications

Sector Typical Q390GJD components
Super-tall towers Column flanges and webs above 60 mm, belt trusses
Long-span roofs Heavy truss chords and supports
Industrial buildings Heavy crane runway girders
Transfer structures Podium transfer girders where plate thickness must drop

D grade covers severe winters, thick welded nodes and members erected in sub-zero weather.

It is the wrong plate for pressure equipment (pressure vessel steel plates), for bare exposed steel (weathering steel plates) or for ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q390GJD from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Xinyu, Valin Xiangtan, Shougang, Puyang and Hongchang when size requires.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
  • Tests: tensile, −20°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill

We ship GB, ASTM, ASME, EN, DIN and JIS plate to the United States, Europe, the Middle East, Southeast Asia, Africa and South America. Q390GJD mostly goes to EPC contractors building Chinese-code projects abroad.

Lead time: stock sizes about 5–7 days; mill rolling about 30–45 days; Z35 or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.

Why Choose SHH STEEL

SHH STEEL is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. For Q390GJD that means real GJ plate at mill price, not relabelled general structural plate.

Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio within the cap, CEV inside the thickness band for the delivery route, and −20°C impact at 47 J or more. If one fails, the plate does not ship as GJ.

We also tell buyers when they are over-specifying. If the plate is under 40 mm and strength is not critical, Q345GJD may be the cheaper answer. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q390GJD steel?
Q390GJD is high-performance building structure steel plate to GB/T 19879. It has 390 MPa minimum yield, a 390–510 MPa yield window from 16 to 100 mm, yield ratio ≤0.83, CEV limits by delivery route and Charpy impact of at least 47 J at −20°C. GJ stands for gao jian, high-performance building steel.
What is the difference between Q390GJD and Q390D?
Q390D (GB/T 1591) guarantees 390 MPa only to 16 mm; minimum yield falls to 380 MPa above 16 mm and 360 MPa above 40 mm, with no yield cap or ratio limit. Q390GJD (GB/T 19879) holds 390–510 MPa from 16 to 100 mm, caps the yield ratio at 0.83 and needs 47 J at −20°C.
When should I specify Q390GJD instead of Q390GJC?
Specify Q390GJD when the lowest service or erection temperature reaches about −20°C, when plate is thick and heavily restrained, or when Z25/Z35 is ordered. D is tested at −20°C (47 J) and its melt is cleaner: C ≤0.18%, P ≤0.020%, S ≤0.010%, against P 0.025% and S 0.015% for C grade.
What delivery conditions are allowed for Q390GJ?
GB/T 19879-2023 lists CR, NR, N and NT, with CEV ≤0.45% to 50 mm, and TMCP or TMCP+T, with CEV ≤0.40% to 50 mm. The route is agreed in the contract and printed on the certificate.
What certificate comes with Q390GJD plate?
Q390GJD ships with an EN 10204 3.1 mill certificate by default, or 3.2 with third-party witness. It shows heat analysis and the elements used for CEV, yield, tensile, yield ratio, elongation, Charpy at −20°C, delivery condition, and Z and UT results when ordered.
What is the ASTM or EN equivalent of Q390GJD?
There is no exact equivalent. EN 10025 has no 390 MPa grade, so Q390GJD is compared with S420N/S420M (one step higher) or S355 (one step lower). ASTM A572 Gr.55 is 380 MPa. None of these caps yield or limits the yield ratio, which GB/T 19879 does at 0.83.

Conclusion

Q390GJD steel plate to GB/T 19879 is building structure plate with 390 MPa minimum yield, a capped yield window, a yield-ratio limit and 47 J impact at −20°C. It shares its chemistry with Q390GJB but proves toughness at its own letter. It is not general structural plate under GB/T 1591.

SHH STEEL supplies Q390GJD with heat analysis, CEV, yield ratio and impact on an EN 10204 3.1 or 3.2 certificate, and adds a product analysis checked to GB/T 222 when you need it. Z15, Z25 or Z35, UT to GB/T 2970, Class B or C tolerance, cutting and blasting are available.

We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.

Send the edition, quality letter, Z level and size list; we confirm mill, delivery route, lead time and price in one reply. Contact SHH STEEL for a mill-direct quotation on Q390GJD building steel plate.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X