GB/T 19879 Q345GJD Building Steel Plate Supplier
What is GB/T 19879 Q345GJD Building Steel Plate?
Q345GJD, also written Q345GJ-D or Q345 GJD, is hot-rolled steel plate for building structures under GB/T 19879-2015. Q means yield, 345 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and D is the quality grade: Charpy V-notch at −20°C, at least 47 J. The 2023 edition of the standard calls the same steel Q355GJD.
The GJ rules are what the structural engineer is paying for. Q345GJD sets a maximum yield as well as a minimum, caps the yield ratio, limits carbon equivalent by thickness and delivery route, and keeps P and S low. The frame then yields where the designer expects.
Q345GJD covers thick column plate in northern cities and heavy welded nodes where the designer wants margin against brittle fracture. The D letter brings the leaner melt (C ≤0.18%, P ≤0.020%, S ≤0.010%) and a −20°C Charpy test at 47 J.
GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. GB/T 19879-2023 renamed Q345GJ to Q355GJ. Minimum yield rose from 345 to 355 MPa, the yield window widened from 110 MPa (345–455) to 120 MPa (355–475), the yield-ratio cap moved from 0.80 to 0.83, and CEV for plate up to 50 mm moved from 0.42% to 0.43%. Chemistry did not change. Sister grades are listed under GB/T 19879, including Q345GJB.
SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q345GJD cut to size with an EN 10204 3.1 or 3.2 certificate.
Material Specification
| Specification element | Requirement | SHH STEEL compliance |
|---|---|---|
| Plate standard | GB/T 19879-2015 Q345GJD, or GB/T 19879-2023 Q355GJD | Confirmed |
| Thickness for Q345GJ | 6 mm – 200 mm | Confirmed |
| Yield strength | 345 MPa min; 345–455 MPa 16–50 mm (2015) / 355–475 MPa 16–100 mm (2023) | Confirmed |
| Tensile strength | 490 – 610 MPa (to 100 mm) | Confirmed |
| Yield ratio | ≤ 0.80 (2015) / ≤ 0.83 (2023) | Printed on MTC |
| Quality grade | D, Charpy V at −20°C, KV2 ≥ 47 J, longitudinal | Confirmed |
| Delivery condition | AR, CR, NR, N or TMCP | As ordered |
| Through-thickness | Z15, Z25 or Z35 to GB/T 5313 | As ordered |
| Dimensions | GB/T 709-2019, thickness tolerance Class B | Confirmed |
| Chemistry report | Heat analysis + CEV; product analysis on request | Confirmed |
| Certificate | EN 10204 3.1 or 3.2 | As ordered |
Grades often confused with it are GB/T 1591 Q355D, EN 10025-2 S355J2 and ASTM A572 Gr.50. None of them carries the GJ yield cap or yield-ratio rule.
Chemical Composition: Heat Analysis and Product Analysis
Read the chemistry of Q345GJD in two layers. Layer one is the heat (ladle) analysis on the certificate, judged against Table 1. Layer two is product analysis on the finished plate, judged against Table 1 plus the GB/T 222 deviations (clause 7.1.4). Mixing the two causes most chemistry disputes we see.
Table 1 below is the heat analysis for Q345GJD. The columns on the right show the quality-grade groups at Q345GJ.
Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %
| Element | Q345GJD heat analysis (%) | Q345GJ B / C | Q345GJ D / E |
|---|---|---|---|
| C, max | 0.18 | 0.20 | 0.18 |
| Si, max | 0.55 | 0.55 | 0.55 |
| Mn, max | 1.60 | 1.60 | 1.60 |
| P, max | 0.020 | 0.025 | 0.020 |
| S, max | 0.010 | 0.015 | 0.010 |
| V, max | 0.150 | 0.150 | 0.150 |
| Nb, max | 0.070 | 0.070 | 0.070 |
| Ti, max | 0.035 | 0.035 | 0.035 |
| Als, min | 0.015 | 0.015 | 0.015 |
| Cr, max | 0.30 | 0.30 | 0.30 |
| Cu, max | 0.30 | 0.30 | 0.30 |
| Ni, max | 0.30 | 0.30 | 0.30 |
| Mo, max | 0.20 | 0.20 | 0.20 |
| V + Nb + Ti, max (if combined) | 0.15 | 0.15 | 0.15 |
Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. V + Nb + Ti, when combined, is limited to 0.15%. These limits are the same in the 2015 and 2023 editions.
B and C grades share one chemistry column. D and E grades tighten carbon to 0.18%, phosphorus to 0.020% and sulfur to 0.010%, because they are tested at −20°C and −40°C.
Table 2. Product analysis limits for Q345GJD, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %
| Element | Heat limit (%) | Permitted deviation, GB/T 222-2025 Table 1 | Q345GJD product analysis limit (%) |
|---|---|---|---|
| C | ≤ 0.18 | +0.02 | ≤ 0.20 |
| Si | ≤ 0.55 | +0.05 | ≤ 0.60 |
| Mn | ≤ 1.60 | +0.06 | ≤ 1.66 |
| P | ≤ 0.020 | +0.005 | ≤ 0.025 |
| S | ≤ 0.010 | +0.005 | ≤ 0.015 |
| V | ≤ 0.150 | +0.02 | ≤ 0.170 |
| Nb | ≤ 0.070 | ±0.005 | ≤ 0.075 (Table 1 lists Nb to 0.060%; agree above that) |
| Ti | ≤ 0.035 | +0.02 | ≤ 0.055 |
| Als | ≥ 0.015 | −0.003 | ≥ 0.012 |
| Cr | ≤ 0.30 | +0.05 | ≤ 0.35 |
| Cu | ≤ 0.30 | +0.05 | ≤ 0.35 |
| Ni | ≤ 0.30 | +0.05 | ≤ 0.35 |
| Mo | ≤ 0.20 | Not listed in Table 1 | Agree in contract (alloy-steel Table 2 would give ≤ 0.21) |
How to read Table 2. The band is chosen by the Table 1 upper limit. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn ≤1.60% falls in the 0.80–1.70% band, so +0.06%. For one heat an element may deviate in one direction only.
GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).
Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.
Mechanical Properties
Values below follow Table 3 and Table 5 of GB/T 19879-2023 for Q355GJ, the 2023 name of Q345GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.
| Thickness | Upper yield ReH (MPa) | Tensile Rm (MPa) | Yield ratio, max | Elongation A, min |
|---|---|---|---|---|
| 6 – 16 mm | ≥ 355 | 490 – 610 | 0.83 | 22% |
| > 16 – 100 mm | 355 – 475 | 490 – 610 | 0.83 | 22% |
| > 100 – 150 mm | 335 – 455 | 470 – 600 | 0.83 | 22% |
| > 150 – 200 mm | 325 – 445 | 470 – 600 | 0.83 | 22% |
For orders to the 2015 edition, Q345GJ uses lower yield ReL and these bands, with yield ratio ≤ 0.80 and A ≥ 22%:
| Thickness (2015) | ReL (MPa) | Rm (MPa) |
|---|---|---|
| 6 – 16 mm | ≥ 345 | 490 – 610 |
| > 16 – 50 mm | 345 – 455 | 490 – 610 |
| > 50 – 100 mm | 335 – 445 | 490 – 610 |
| > 100 – 150 mm | 325 – 435 | 470 – 610 |
| > 150 – 200 mm | 305 – 415 | 470 – 610 |
| Test | Q345GJD requirement |
|---|---|
| Charpy V-notch, longitudinal | −20°C, KV2 ≥ 47 J, average of 3 |
| Single value | One value may fall below the average requirement, not below 70% of it (GB/T 17505) |
| Sub-size specimens | 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy |
| 180° bend | Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2) |
| Through-thickness (≥ 15 mm) | Z15, Z25 or Z35 to GB/T 5313, when ordered |
Density for theoretical weight is 7.85 g/cm³.
Q345GJD vs Q355D and Q345D: Building Plate or General Structural Plate?
Q345D was the GB/T 1591-2008 name. GB/T 1591-2018 replaced it with GB/T 1591 Q355D. Q345GJD is a different book again: GB/T 19879, written for building frames. Buyers mix the three up every week.
The general structural grade is sold on its minimum yield. The building grade is sold on control: a yield ceiling, a yield-ratio cap, a CEV limit, lower P and S, and 47 J impact. In a seismic frame those rules decide where the steel yields first.
| Property | Q355D (GB/T 1591-2018) | Q345GJD (GB/T 19879-2015) | Q355GJD (GB/T 19879-2023) |
|---|---|---|---|
| Yield at 16 mm | 355 MPa | 345 MPa | 355 MPa |
| Yield at 40–63 mm | 335 MPa min | 345–455 MPa (to 50 mm) | 355–475 MPa |
| Yield at 80–100 mm | 315 MPa min | 335–445 MPa | 355–475 MPa |
| Yield upper limit | None | Yes (110 MPa window) | Yes (120 MPa window) |
| Yield ratio | No limit | ≤ 0.80 | ≤ 0.83 |
| Tensile, to 100 mm | 470 – 630 MPa | 490 – 610 MPa | 490 – 610 MPa |
| Impact | −20°C, 34 J | −20°C, 47 J | −20°C, 47 J |
| P / S, max | Per GB/T 1591 grade | 0.020 / 0.010% | 0.020 / 0.010% |
| Maximum thickness | 250 mm (AR tables) | 200 mm | 200 mm |
Q345GJD can replace Q355D in almost every case. Q355D cannot replace Q345GJD: its certificate never reports a yield ratio or a GJ CEV band.
EN 10025-2 S355J2 is the European −20°C comparison at 27 J. It has no yield cap and is not a GJ substitute without the designer’s sign-off.
Q345GJD vs Q355GJD: What Changed in GB/T 19879-2023
GB/T 19879-2023 replaced the 2015 edition on 1 April 2024 and renamed Q345GJ to Q355GJ. Chemistry is identical. Strength and ratio rules are not, and that is what decides whether one certificate can serve both names.
| Rule | Q345GJD (2015) | Q355GJD (2023) |
|---|---|---|
| Yield measured as | Lower yield ReL | Upper yield ReH |
| 6 – 16 mm | ≥ 345 MPa | ≥ 355 MPa |
| > 16 – 50 mm | 345 – 455 MPa | 355 – 475 MPa |
| > 50 – 100 mm | 335 – 445 MPa | 355 – 475 MPa |
| > 100 – 150 mm | 325 – 435 MPa | 335 – 455 MPa |
| > 150 – 200 mm | 305 – 415 MPa | 325 – 445 MPa |
| Tensile, to 100 mm | 490 – 610 MPa | 490 – 610 MPa |
| Yield ratio | ≤ 0.80 | ≤ 0.83 |
| CEV ≤ 50 mm (AR/CR/N) | 0.42% | 0.43% |
| Impact | −20°C, 47 J | −20°C, 47 J |
| Delivery codes | WAR, WCR, N, TMCP | AR, CR, NR, N, TMCP |
The trap is the overlap. A Q355GJ plate at 470 MPa yield or a 0.82 ratio passes 2023 but fails a 2015 Q345GJ order. A Q345GJ plate at 350 MPa passes 2015 but fails 2023.
When a drawing still says Q345GJD, we ask which edition the reviewer will use. If both, we dual-certify only plate that sits inside both windows: 355–455 MPa yield (to 50 mm) and a ratio of 0.80 or lower.
Q345GJB, Q345GJC, Q345GJD or Q345GJE: Which Quality Grade?
| Grade | Impact temperature | Energy, min | C / P / S max (%) | Typical use |
|---|---|---|---|---|
| Q345GJB | +20°C | 47 J | 0.20 / 0.025 / 0.015 | Heated interiors, mild climates |
| Q345GJC | 0°C | 47 J | 0.20 / 0.025 / 0.015 | Cold regions, exposed frames |
| Q345GJD | −20°C | 47 J | 0.18 / 0.020 / 0.010 | Severe winters, thick welded nodes |
| Q345GJE | −40°C | 47 J | 0.18 / 0.020 / 0.010 | Arctic and low-temperature sites |
Strength, yield ratio and CEV do not change from B to E. Only the impact temperature and the D/E chemistry move. Over-specifying the letter costs money; under-specifying it costs safety. Use the design temperature.
Q345GJD is the letter for −20°C design temperatures, and the one we suggest when the plate is thick and restrained. For the same letter at another strength level: one level up, Q390GJD; one level down, Q235GJD.
Q345GJDZ15, Q345GJDZ25 and Q345GJDZ35: Through-Thickness Plate
Through-thickness ductility matters wherever the load path runs across the plate: column flanges at moment connections, cruciform nodes, anchor base plates. GB/T 5313 measures it as reduction of area on short-transverse specimens.
The designation adds the Z level to the grade, for example Q345GJDZ25. Z tests apply to plate 15 mm and thicker and follow GB/T 5313-2023.
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
The D melt already caps S at 0.010%, the Z15 limit, so Z25 and Z35 are the levels that change the steelmaking.
GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.
Z35 on every plate is an easy line to write and an expensive one to buy. Let the joint detail decide where it goes.
Equivalent Material Grades
The nearest foreign building steel is JIS G3136 SN490, which also caps yield and yield ratio. ASTM A992 is the US seismic shape grade with a 0.85 ratio cap; it is a section standard, not plate.
| Designation | Region | Standard | Notes |
|---|---|---|---|
| Q345GJD | China | GB/T 19879-2015 | Grade on this page |
| Q355GJD | China | GB/T 19879-2023 | Current name; see the 2015/2023 table |
| SN490C | Japan | JIS G3136 | Closest building steel: yield range, ratio ≤ 0.80, Z option |
| EN 10025-2 S355J2 | Europe | EN 10025-2 | Strength and temperature comparison only |
| EN 10025-2 S355K2 | Europe | EN 10025-2 | 40 J / 27 J at −20°C |
| JIS G3106 SM490C | Japan | JIS G3106 | No yield-ratio rule |
| ASTM A572 Gr.50 | USA | ASTM A572 | 345 MPa; no impact or ratio rule |
| ASTM A709 Grade 50 | USA | ASTM A709 | Bridge grade; toughness by zone |
| DIN 17100 St52-3 | Germany | DIN 17100 (withdrawn) | Legacy name |
For plate certificates on EN projects, EN 10025-2 or EN 10025-3 plate with EN 10164 Z grades is the usual route. We dual-certify only when both books pass, and say so on the MTC.
Weldability
GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q345GJD certificate:
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B
| Delivery condition | CEV ≤ 50 mm | CEV > 50 – 100 mm | CEV > 100 – 150 mm | CEV > 150 – 200 mm | Pcm ≤ 50 mm | Pcm > 50 – 100 mm | Pcm > 100 – 150 mm | Pcm > 150 – 200 mm |
|---|---|---|---|---|---|---|---|---|
| AR, CR, NR, N (2023) | 0.43 | 0.45 | 0.46 | 0.47 | 0.26 | 0.29 | 0.30 | 0.30 |
| TMCP (2023) | 0.38 | 0.40 | By agreement | — | 0.24 | 0.26 | — | — |
| WAR, WCR, N (2015, Q345GJ) | 0.42 | 0.44 | 0.46 | 0.47 | — | — | — | — |
At 0.43% CEV (2023, ≤50 mm) Q355GJ welds with ordinary structural procedures. Preheat climbs with thickness and restraint; plate over 50 mm in box columns is where most shops start preheating as routine.
The D letter helps: carbon is capped at 0.18% and P and S are lower, which reduces hot-cracking and HAZ embrittlement risk.
Typical consumables: E50-class low-hydrogen electrodes (E5015/E5016) or ER50-6 wire; AWS E7018 / ER70S-6. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.
Heat Treatment and Delivery Condition
Q345GJD/Q355GJD may be delivered AR, CR, NR or N, or TMCP. In the 2015 text the codes were WAR (hot rolled), WCR (controlled rolled), N and TMCP.
Up to about 60 mm most plate ships CR or TMCP. Thick column plate and Z35 plate often ship normalized, which evens out properties through the thickness.
The GB/T 1591 grades with fixed delivery routes are GB/T 1591 Q355ND (normalized) and GB/T 1591 Q355MD (TMCP); compare with EN 10025-3 S355N and EN 10025-4 S355M in Europe.
Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.
Dimensions
What we roll and cut in Q345GJD:
- Thickness: 6 mm – 200 mm; most orders 10 mm – 120 mm
- Width: 1500 mm – 3000 mm standard; wider by mill confirmation
- Length: 3000 mm – 12000 mm; longer by enquiry
- Edge: mill edge or cut edge
- Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³
Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.
Tolerances
For Q345GJD, thickness tolerance follows GB/T 709-2019 Class B unless the order says otherwise: −0.30 mm on the minus side at every thickness, with the plus side shown below. Zero-minus Class C can be agreed.
| Nominal thickness (mm) | Width ≤ 1500 mm | Width > 1500 – 2500 mm |
|---|---|---|
| > 8 – 15 | −0.30 / +0.80 | −0.30 / +1.00 |
| > 15 – 25 | −0.30 / +1.00 | −0.30 / +1.20 |
| > 25 – 40 | −0.30 / +1.10 | −0.30 / +1.30 |
| > 40 – 60 | −0.30 / +1.30 | −0.30 / +1.50 |
| > 60 – 100 | −0.30 / +1.50 | −0.30 / +1.80 |
| > 100 – 150 | −0.30 / +2.10 | −0.30 / +2.50 |
Plate over 150 mm follows the heavier rows of GB/T 709; we state the figures on the offer. Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.
Supplementary Requirements
Q345GJD already fixes strength, yield ratio, CEV and −20°C impact. Anything more goes on the purchase order.
- Edition: GB/T 19879-2015 (Q345GJ) or -2023 (Q355GJ). Never write only Q345.
- Product analysis: ask for a second chemistry column checked to GB/T 222.
- Through-thickness: add Z15, Z25 or Z35, e.g. Q345GJDZ25.
- Delivery condition: name it (AR, CR, NR, N or TMCP) if the welding procedure depends on it.
- Ultrasonic testing beyond Z plates: GB/T 2970 class, or EN 10160 / ASTM A578.
- Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the D letter.
- Tolerance: Class C for zero minus.
- Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.
Q345GJD Price Factors and How to Order
When you compare Q345GJD offers, compare extras line by line. These are the items that move the price.
| Cost driver | Effect on price |
|---|---|
| GJ grade over general Q345 plate | Grade extra for cleaner steel, yield control and CEV |
| Quality letter D | Extra for −20°C testing and the cleaner D melt |
| Delivery route | N and TMCP carry extras over AR/CR |
| Thickness | Thin and very thick plate carry size extras; 10–60 mm is usually cheapest |
| Z15 / Z25 / Z35 | Desulfurization, plate-by-plate Z test and UT; Z35 costs most |
| Width and length | Over 3000 mm wide or 12 m long needs mill confirmation |
| Quantity per size | Mill rolling minimums per size; small lots come from stock or combined rolling |
| Inspection and cutting | 3.2 witness, profile cutting, blasting and priming are quoted per item |
To get a firm quote in one round, send:
- Grade and edition, e.g. Q345GJDZ25 to GB/T 19879-2015
- Thickness × width × length and pieces or tonnes
- Delivery route, UT standard and class
- Certificate type and inspector
- Destination port and Incoterm
We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q345GJE.
Applications
| Sector | Typical Q345GJD components |
|---|---|
| High-rise towers | Box and H column plates, transfer girders, outrigger webs |
| Airports and stadiums | Long-span roof trusses, tree columns, node plates |
| Seismic frames | Beam-to-column panel zones, links, brace gussets |
| Industrial buildings | Heavy crane girders, column bases |
| Bridges in buildings | Skybridges, podium transfer trusses |
D grade covers severe winters, thick welded nodes and members erected in sub-zero weather.
It is the wrong plate for pressure equipment (pressure vessel steel plates), for bare exposed steel (weathering steel plates) or for ship hulls (shipbuilding steel plates).
Supply Capability and Global Delivery
SHH STEEL sources Q345GJD from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Xinyu, Valin Xiangtan, Shougang, Puyang and Hongchang when size requires.
- Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
- Tests: tensile, −20°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
- Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
- Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
- Marking: steel-stamped and paint-marked with grade, heat, size and mill
Our Q345GJD exports go where Chinese design codes go: high-rise, airport and industrial projects run by EPC contractors abroad. The same team ships GB, ASTM, ASME, EN, DIN and JIS plate worldwide.
Lead time: stock sizes about 5–7 days; mill rolling about 30–45 days; Z35 or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.
Why Choose SHH STEEL
SHH STEEL is mill-direct: steel manufacturer and exporter and global steel mill sourcing partner, China origin. Every Q345GJD plate we ship carries the original mill heat number.
Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio within the cap, CEV inside the thickness band for the delivery route, and −20°C impact at 47 J or more. If one fails, the plate does not ship as GJ.
We also tell buyers when they are over-specifying. If the member is outside the lateral system, GB/T 1591 Q355D may be enough, and we will tell you. Browse more structural steel plates and high strength low alloy plates.
FAQ
-
What is Q345GJD steel?
- Q345GJD is building structure steel plate to GB/T 19879-2015 with 345 MPa minimum yield, a 110 MPa yield window, yield ratio ≤0.80, CEV limits and Charpy impact of at least 47 J at −20°C. GB/T 19879-2023 renamed it Q355GJD, with 355–475 MPa yield and a 0.83 ratio cap.
-
What is the difference between Q345GJD and Q355D?
- Q355D is general structural plate to GB/T 1591-2018 with a minimum yield that falls with thickness and no yield cap or ratio limit. Q345GJD is building plate to GB/T 19879 with a capped yield window, a yield ratio of 0.80 (2015) or 0.83 (Q355GJD, 2023), CEV limits and 47 J at −20°C. Q345GJD can replace Q355D; the reverse needs designer approval.
-
When should I specify Q345GJD instead of Q345GJC?
- Specify Q345GJD when the lowest service or erection temperature reaches about −20°C, when plate is thick and heavily restrained, or when Z25/Z35 is ordered. D is tested at −20°C (47 J) and its melt is cleaner: C ≤0.18%, P ≤0.020%, S ≤0.010%, against P 0.025% and S 0.015% for C grade.
-
What is the yield ratio of Q345GJ?
- GB/T 19879-2015 limits the Q345GJ yield ratio (ReL/Rm) to 0.80 for all thicknesses up to 200 mm. The renamed Q355GJ in GB/T 19879-2023 allows up to 0.83 (ReH/Rm). The ratio is printed on the mill certificate.
-
How is Q345GJD priced?
- Q345GJD is priced as a base plate price plus extras: GJ grade extra, D-letter impact extra, thickness and width extras, delivery route (AR, CR, NR, N or TMCP), Z15/Z25/Z35, UT class, inspection and cutting. Quantity per size matters because mills set rolling minimums.
-
What is the ASTM or EN equivalent of Q345GJD?
- The current Chinese name is Q355GJD (GB/T 19879-2023). Abroad, the closest building steel is JIS G3136 SN490C. EN 10025-2 S355J2 and ASTM A572 Gr.50 match strength only: they have no yield cap or yield-ratio limit, so they are not direct substitutes.
Conclusion
Q345GJD steel plate to GB/T 19879 is building structure plate with 345 MPa (2015) or 355 MPa (2023, as Q355GJD) minimum yield, a capped yield window, a yield-ratio limit and 47 J impact at −20°C. It shares its chemistry with Q345GJB but proves toughness at its own letter. It is not general structural plate under GB/T 1591.
SHH STEEL delivers Q345GJD with the full GJ data set on an EN 10204 3.1 or 3.2 certificate: heat analysis, CEV, yield, yield ratio and impact. On request we add product analysis to GB/T 222, Z15, Z25 or Z35, GB/T 2970 UT, Class C tolerance, cutting and blasting.
We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.
Ready to order? Send the drawing or cutting list, the certificate type and the destination port. Our engineers check the edition, letter and Z level before we quote, so the offer matches the drawing. Contact SHH STEEL for a mill-direct quotation on Q345GJD building steel plate.