What is GB/T 19879 Q690GJE Building Steel Plate?
Q690GJE, also written Q690GJ-E or Q690 GJE, is high-strength plate for building structures under GB/T 19879-2023. Q means yield, 690 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and E is the quality grade: Charpy V-notch at −40°C, at least 47 J.
The GJ rules still apply at this strength. Q690GJE has a yield ceiling of 860 MPa above 20 mm, a CEV cap of 0.60% for QT plate and low P and S. Unlike Q235GJ–Q460GJ, it is made only by quenching and tempering or TMCP, only from 12 to 50 mm, and its yield ratio is agreed in the contract.
Q690GJE is 690 MPa building plate with 47 J at −40°C. It is a QT product in practice, and the welding procedure, not the plate, is usually the limiting factor on site.
GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. Q690GJ entered GB/T 19879 in the 2015 edition; the 2005 edition stopped at Q460GJ. In 2015 the grade covered 12–40 mm and reported ReL. The 2023 edition keeps the same chemistry, extends the range to 50 mm, reports ReH, and sets 55 J at 0°C for C and 47 J at −20°C / −40°C for D and E. Sister grades are listed under GB/T 19879, including Q690GJC.
SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q690GJE cut to size with an EN 10204 3.1 or 3.2 certificate.
Material Specification
| Specification element | Requirement | SHH STEEL compliance |
|---|---|---|
| Plate standard | GB/T 19879-2023 Q690GJE (GB/T 19879-2015 when the drawing names it) | Confirmed |
| Thickness for Q690GJ | 12 mm – 50 mm | Confirmed |
| Yield strength | 690 MPa min; 690 – 860 MPa above 20 mm | Confirmed |
| Tensile strength | 770 – 940 MPa | Confirmed |
| Yield ratio | By agreement; we print it on the MTC | Printed on MTC |
| Quality grade | E, Charpy V at −40°C, KV2 ≥ 47 J, longitudinal | Confirmed |
| Delivery condition | QT, TMCP or TMCP+T | As ordered |
| Through-thickness | Z15, Z25 or Z35 to GB/T 5313 | As ordered |
| Dimensions | GB/T 709-2019, thickness tolerance Class B | Confirmed |
| Chemistry report | Heat analysis + CEV; product analysis on request | Confirmed |
| Certificate | EN 10204 3.1 or 3.2 | As ordered |
Grades often confused with it are GB/T 16270 Q690E and GB/T 1591 Q690ME. None of them carries the GJ yield cap.
Chemical Composition: Heat Analysis and Product Analysis
Buyers often reject plate because a third-party lab reads 0.02% more carbon than the MTC. That is usually not a failure. Table 1 is the heat (ladle) limit; plate drilled after rolling is judged as product analysis, with the tolerances of GB/T 222 that clause 7.1.4 calls up.
Table 1 below is the heat analysis for Q690GJE. The columns on the right show the quality-grade groups at Q690GJ.
Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %
| Element | Q690GJE heat analysis (%) | Q690GJ C | Q690GJ D / E |
|---|---|---|---|
| C, max | 0.18 | 0.18 | 0.18 |
| Si, max | 0.60 | 0.60 | 0.60 |
| Mn, max | 2.20 | 2.20 | 2.20 |
| P, max | 0.020 | 0.025 | 0.020 |
| S, max | 0.010 | 0.015 | 0.010 |
| V, max | 0.120 | 0.120 | 0.120 |
| Nb, max | 0.110 | 0.110 | 0.110 |
| Ti, max | 0.030 | 0.030 | 0.030 |
| Als, min | 0.015 | 0.015 | 0.015 |
| Cr, max | 1.20 | 1.20 | 1.20 |
| Cu, max | 0.50 | 0.50 | 0.50 |
| Ni, max | 2.00 | 2.00 | 2.00 |
| Mo, max | 0.60 | 0.60 | 0.60 |
| B, max (if added) | 0.003 | 0.003 | 0.003 |
Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. When boron is added, and for any QT plate, B ≤ 0.003%. These limits are the same in the 2015 and 2023 editions.
The C and D/E columns differ only in P and S: the D and E letters tighten P to 0.020% and S to 0.010%. Carbon stays at 0.18% for every quality letter at this level.
Table 2. Product analysis limits for Q690GJE, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %
| Element | Heat limit (%) | Permitted deviation, GB/T 222-2025 Table 2 (alloy steel) | Q690GJE product analysis limit (%) |
|---|---|---|---|
| C | ≤ 0.18 | +0.01 | ≤ 0.19 |
| Si | ≤ 0.60 | +0.04 | ≤ 0.64 |
| Mn | ≤ 2.20 | +0.05 | ≤ 2.25 |
| P | ≤ 0.020 | +0.005 | ≤ 0.025 |
| S | ≤ 0.010 | +0.005 | ≤ 0.015 |
| V | ≤ 0.120 | +0.03 | ≤ 0.150 |
| Nb | ≤ 0.110 | Agree in contract | Agree in contract |
| Ti | ≤ 0.030 | +0.02 | ≤ 0.050 |
| Als | ≥ 0.015 | ±0.005 band (Al ≤ 0.10%) | Agree in contract |
| Cr | ≤ 1.20 | +0.05 | ≤ 1.25 |
| Cu | ≤ 0.50 | +0.03 | ≤ 0.53 |
| Ni | ≤ 2.00 | +0.05 | ≤ 2.05 |
| Mo | ≤ 0.60 | +0.02 | ≤ 0.62 |
| B (if added) | ≤ 0.003 | Agree in contract | Agree in contract |
How to read Table 2. Q500GJ–Q690GJ heats carry Ni, Cr, Mo and often B for hardenability, which normally classes them as alloy steel, so the alloy-steel table of GB/T 222 applies. For Q690GJE, Mn ≤2.20% sits in the 2.00–3.00% band (±0.05), and Ni ≤2.00% in the 1.00–2.00% band (±0.05). GB/T 222 clause 5.4 says one steel uses one table only, so the certificate should state which table was applied.
GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).
Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.
Mechanical Properties
Values below follow Table 4 and Table 5 of GB/T 19879-2023 for Q690GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.
| Thickness | Upper yield ReH (MPa) | Tensile Rm (MPa) | Yield ratio, max | Elongation A, min |
|---|---|---|---|---|
| 12 – 20 mm | ≥ 690 | 770 – 940 | By agreement | 14% |
| > 20 – 50 mm | 690 – 860 | 770 – 940 | By agreement | 14% |
Below 20 mm only the 690 MPa minimum applies; from 20 to 50 mm the 690 – 860 MPa window applies. Write the yield-ratio limit into the contract; GB/T 19879-2023 leaves it to agreement for this grade.
| Test | Q690GJE requirement |
|---|---|
| Charpy V-notch, longitudinal | −40°C, KV2 ≥ 47 J, average of 3 |
| Single value | One value may fall below the average requirement, not below 70% of it (GB/T 17505) |
| Sub-size specimens | 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy |
| 180° bend | Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2) |
| Through-thickness (≥ 15 mm) | Z15, Z25 or Z35 to GB/T 5313, when ordered |
Density for theoretical weight is 7.85 g/cm³.
Q690GJE vs S690QL and GB/T 16270 Q690E: What Building Plate Adds
At 690 MPa the plate itself is not unusual. GB/T 16270 Q690E and EN 10025-6 S690QL are standard QT products. What Q690GJE adds is a building-steel frame around them: a yield ceiling of 860 MPa above 20 mm, a tensile floor of 770 MPa, a CEV cap written into the standard, and Charpy at the GB quality letter.
The trade-off is thickness. GB/T 19879 stops at 50 mm for this grade; EN 10025-6 and GB/T 16270 go much thicker.
| Property | S690QL (EN 10025-6) | Q690E (GB/T 16270) | Q690GJE (GB/T 19879-2023) |
|---|---|---|---|
| Delivery | QT | QT | QT or TMCP |
| Thickness range | to 150 mm | to 150 mm | 12 – 50 mm |
| Yield, ≤ 50 mm | ≥ 690 MPa | ≥ 690 MPa | 690 – 860 MPa above 20 mm |
| Tensile, ≤ 50 mm | 770 – 940 MPa | Per GB/T 16270 | 770 – 940 MPa |
| Yield ratio | No limit | No limit | By agreement (write it on the order) |
| Impact | −20°C / −40°C (QL) | −40°C | −40°C, 47 J |
| Elongation A | 14% | Per GB/T 16270 | 14% |
| CEV ≤ 50 mm | Per EN 10025-6 | Per GB/T 16270 | 0.60% QT / 0.50% TMCP |
If a member is thicker than 50 mm, it cannot be Q690GJE. The designer either splits the plate, or moves to GB/T 16270 Q690E or the EN grade with project-specific yield-cap rules. The TMCP comparison in GB/T 1591 is GB/T 1591 Q690ME.
QT or TMCP? Delivery Condition, CEV and Weldability of Q690GJE
| Route | CEV max (≤ 50 mm) | Pcm max (≤ 50 mm) | Typical use |
|---|---|---|---|
| QT (incl. direct quench) | 0.60% | By agreement | Full strength through 50 mm; highest alloy |
| TMCP, TMCP+T | 0.50% | 0.30% (reference value) | Leaner chemistry; easier welding on thinner plate |
Q690GJ cannot be made as plain hot-rolled or normalized plate; GB/T 19879-2023 lists only QT and TMCP routes for it. The two routes are not equal at the welding bay.
QT Q690GJE carries up to 0.60% CEV, because the mill adds Mn, Ni, Cr, Mo and sometimes B for hardenability. TMCP plate is capped at 0.50%. For welding procedure purposes those are different steels.
The 2023 edition lets TMCP plate ship against Pcm instead of CEV only when buyer and mill agree in the contract. The Pcm figure in the standard for TMCP plate is given for reference.
Q690GJC, Q690GJD or Q690GJE: Which Quality Grade?
| Grade | Impact temperature | Energy, min | C / P / S max (%) | Typical use |
|---|---|---|---|---|
| Q690GJC | 0°C | 55 J | 0.18 / 0.025 / 0.015 | Cold regions, exposed frames |
| Q690GJD | −20°C | 47 J | 0.18 / 0.020 / 0.010 | Severe winters, thick welded nodes |
| Q690GJE | −40°C | 47 J | 0.18 / 0.020 / 0.010 | Arctic and low-temperature sites |
Strength, yield window and CEV do not change from C to E. Only the impact temperature, the C-grade energy (55 J) and the D/E P and S limits move. Choose the letter from the site climate and plate thickness, not from habit.
Q690GJE is the coldest letter in GB/T 19879; there is no F grade in this standard. For the same letter at another strength level: one level down, Q620GJE.
Q690GJEZ15, Q690GJEZ25 and Q690GJEZ35: Through-Thickness Plate
A weld on the face of a thick plate shrinks and pulls the plate apart through its thickness. If the steel holds sulfide stringers, it tears in steps. Z15, Z25 and Z35 prove through-thickness ductility with a short-transverse tensile test.
The designation adds the Z level to the grade, for example Q690GJEZ25. Z tests apply to plate 15–50 mm and follow GB/T 5313-2023.
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
The E melt already caps S at 0.010%, the Z15 limit, so Z25 and Z35 are the levels that change the steelmaking.
GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.
Most projects need Z only on flange and diaphragm plates over about 25–40 mm. Put the Z level on those items alone and keep the rest standard Q690GJE.
Equivalent Material Grades
At 690 MPa every foreign comparison is a QT plate standard, not a building-steel standard. They match strength and toughness temperature. None of them sets a yield ceiling or a yield-ratio rule.
| Designation | Region | Standard | Notes |
|---|---|---|---|
| Q690GJE | China | GB/T 19879-2023 | Grade on this page; 12–50 mm |
| EN 10025-6 S690QL | Europe | EN 10025-6 | QT; closest strength match |
| EN 10025-6 S690QL1 | Europe | EN 10025-6 | Colder sub-grade |
| GB/T 16270 Q690E | China | GB/T 16270 | QT structural plate; thicker sizes |
| GB/T 1591 Q690ME | China | GB/T 1591-2018 | TMCP route |
| ASTM A514 Grade Q | USA | ASTM A514 | 690 MPa QT; to 65 mm at full yield |
| ASTM A709 HPS 100W | USA | ASTM A709 | 690 MPa bridge plate |
See EN 10025-6 and GB/T 16270 for thicker or non-building QT plate.
Weldability
GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q690GJE certificate:
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B
| Delivery condition | CEV, max (≤ 50 mm) | Pcm, max (≤ 50 mm) |
|---|---|---|
| QT (quenched + tempered, incl. direct quench) | 0.60 | By agreement |
| TMCP, TMCP+T | 0.50 | 0.30 (for reference) |
Q690GJ is the hardest grade in the standard to weld. A published Q690GJ manual-arc procedure uses at least 120°C preheat and 120–170°C interpass; treat that as a reference point and qualify your own.
The impact test on the E letter is at −40°C. Qualify the HAZ Charpy at that temperature, not only the weld metal.
Typical consumables: E76- or E78-class low-hydrogen consumables (GB/T 5118 / GB/T 8110) for full-strength butt welds against the 770 MPa tensile floor; lower-strength fillers only where the designer accepts under-matching. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.
Heat Treatment and Delivery Condition
Q690GJE is delivered QT (quenched and tempered, including in-line direct quenching) or TMCP / TMCP+T. Hot-rolled and normalized delivery are not allowed for this grade.
Most building orders at this level ship QT. TMCP plate is possible on thinner sizes and gives a lower CEV cap, but not every mill can hold the GJ yield ceiling on TMCP plate up to 50 mm.
Tempering temperature and time are mill data. We ask for them on the MTC when the fabricator plans post-weld heat treatment, so that PWHT stays below the tempering temperature. QT references: GB/T 16270 Q690E and EN 10025-6 S690QL.
Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.
Dimensions
Typical Q690GJE dimensions on our offers:
- Thickness: 12 mm – 50 mm
- Width: 1500 mm – 3000 mm standard; wider by mill confirmation; QT width depends on the mill’s quench line
- Length: 3000 mm – 12000 mm; longer by enquiry
- Edge: mill edge or cut edge
- Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³
Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.
Tolerances
GB/T 709-2019 governs Q690GJE thickness, width, length and flatness. Under Class B, the default, plate may be up to 0.30 mm thin and the plus side grows with thickness and width. Class C gives zero minus by agreement.
| Nominal thickness (mm) | Width ≤ 1500 mm | Width > 1500 – 2500 mm |
|---|---|---|
| > 8 – 15 | −0.30 / +0.80 | −0.30 / +1.00 |
| > 15 – 25 | −0.30 / +1.00 | −0.30 / +1.20 |
| > 25 – 40 | −0.30 / +1.10 | −0.30 / +1.30 |
| > 40 – 60 | −0.30 / +1.30 | −0.30 / +1.50 |
Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.
Supplementary Requirements
Q690GJE already fixes strength, yield window, CEV and −40°C impact. Anything more goes on the purchase order.
- Edition: GB/T 19879-2023 or -2015. Never write only Q690.
- Product analysis: ask for a second chemistry column checked to GB/T 222.
- Through-thickness: add Z15, Z25 or Z35, e.g. Q690GJEZ25.
- Delivery route: QT or TMCP, and the CEV/Pcm basis.
- Yield ratio: the designer’s limit, since the standard leaves it to agreement.
- Tempering data on the MTC if the fabricator plans post-weld heat treatment.
- Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the E letter.
- Tolerance: Class C for zero minus.
- Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.
Q690GJE Price Factors and How to Order
There is no single Q690GJE price. Mills price GJ plate as base plus extras, and the order details set the extras.
| Cost driver | Effect on price |
|---|---|
| GJ grade over general Q690 plate | Grade extra for cleaner steel, yield control and CEV |
| Quality letter E | Highest letter extra: −40°C testing, cleaner melt, more retest risk |
| Delivery route | QT line time is the main cost driver at this level |
| Thickness | 12–20 mm and 40–50 mm carry the most care; 20–40 mm is the core range |
| Z15 / Z25 / Z35 | Desulfurization, plate-by-plate Z test and UT; Z35 costs most |
| Width and length | Over 3000 mm wide or 12 m long needs mill confirmation |
| Quantity per size | Mill rolling minimums per size; small lots come from stock or combined rolling |
| Inspection and cutting | 3.2 witness, profile cutting, blasting and priming are quoted per item |
To get a firm quote in one round, send:
- Grade and edition, e.g. Q690GJEZ25 to GB/T 19879-2023
- Thickness × width × length and pieces or tonnes
- Delivery route, UT standard and class
- Certificate type and inspector
- Destination port and Incoterm
We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q690GJD.
Applications
| Sector | Typical Q690GJE components |
|---|---|
| Long-span roofs | Compression chords and diagonals where weight governs |
| Tall buildings | Outrigger and belt truss members, hanger plates |
| Heavy industrial buildings | Crane-runway and support members |
| Special structures | Members where crane capacity or connection size limits plate thickness |
E grade is for the coldest sites and for owners who specify −40°C for every primary member.
It is not boiler or pressure-vessel plate (pressure vessel steel plates), and members thicker than 50 mm move to GB/T 16270 or EN 10025-6.
Supply Capability and Global Delivery
SHH STEEL sources Q690GJE from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Valin Xiangtan and Shougang QT lines.
- Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
- Tests: tensile, −40°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
- Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
- Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
- Marking: steel-stamped and paint-marked with grade, heat, size and mill
Buyers of Q690GJE are usually EPC contractors and fabricators working to Chinese drawings overseas. We ship to the United States, Europe, the Middle East, Southeast Asia, Africa and South America.
QT plate is rolled and heat treated to order: about 45–60 days; 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.
Why Choose SHH STEEL
As a steel manufacturer and exporter and global steel mill sourcing partner, SHH STEEL buys Q690GJE straight from GJ-qualified mills, China origin. No relabelled general plate, no mixed heats.
Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio inside the agreed limit, CEV inside the thickness band for the delivery route, and −40°C impact at 47 J or more. If one fails, the plate does not ship as GJ.
We also tell buyers when they are over-specifying. If a member is thicker than 50 mm, we tell you before quoting: it cannot be Q690GJE. Browse more structural steel plates and high strength low alloy plates.
FAQ
-
What is Q690GJE steel?
- Q690GJE is high-strength building structure steel plate to GB/T 19879-2023, delivered quenched and tempered or TMCP in 12–50 mm. It has 690 MPa minimum yield, 690–860 MPa yield above 20 mm, 770 – 940 MPa tensile, a CEV cap of 0.60% (QT) and Charpy impact of at least 47 J at −40°C.
-
What is the difference between Q690GJE and S690QL?
- S690QL (EN 10025-6) is QT plate with ≥690 MPa yield up to 50 mm, no yield ceiling and no yield-ratio rule, made to 150 mm. Q690GJE (GB/T 19879-2023) is QT or TMCP building plate, 12–50 mm, with 690–860 MPa yield above 20 mm, 770 – 940 MPa tensile, a CEV cap of 0.60% (QT) and 47 J at −40°C.
-
Is Q690GJE suitable for −40°C service?
- Yes. Q690GJE is Charpy tested at −40°C and must average at least 47 J on longitudinal specimens. GB/T 19879 has no colder letter, so for design temperatures below −40°C look at GB/T 16270 Q690F or EN 10025-6 S690QL1 (−60°C) and check the yield-cap rules separately.
-
Is Q690GJ available thicker than 50 mm?
- Not under GB/T 19879. The 2023 edition caps Q690GJ at 50 mm (the 2015 edition at 40 mm). For thicker 690 MPa plate, use GB/T 16270 Q690 or EN 10025-6 S690Q/QL, and add yield-ceiling rules to the contract if the design needs them.
-
What certificate comes with Q690GJE plate?
- Q690GJE ships with an EN 10204 3.1 mill certificate by default, or 3.2 with third-party witness. It shows heat analysis and the elements used for CEV, yield, tensile, yield ratio, elongation, Charpy at −40°C, delivery condition, and Z and UT results when ordered.
-
What is the ASTM or EN equivalent of Q690GJE?
- The closest European grade is EN 10025-6 S690QL; the closest Chinese non-building grades are GB/T 16270 Q690E (QT) and GB/T 1591 Q690ME (TMCP). In the US, ASTM A514 is the 690 MPa QT plate. They match strength only: Q690GJE adds a 860 MPa yield ceiling, a CEV cap and a 50 mm thickness limit.
Conclusion
Q690GJE steel plate to GB/T 19879 is building structure plate with 690 MPa minimum yield, a capped yield window, a yield ratio agreed in the contract and 47 J impact at −40°C. It shares its chemistry with Q690GJC but proves toughness at its own letter. It is not general structural plate under GB/T 1591 or GB/T 16270.
With SHH STEEL the Q690GJE certificate is complete: heat chemistry, CEV, yield, tensile, yield ratio and Charpy impact, to EN 10204 3.1 or 3.2. Add product analysis to GB/T 222, a Z15, Z25 or Z35 level, a GB/T 2970 UT class, Class C tolerance or profile cutting as the project needs.
We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.