GB/T 714 Q370qD bridge steel plate stacked at SHH STEEL warehouse

GB/T 714 Q370qD Bridge Steel Plate Supplier

GB/T 714 Q370qD is bridge structural steel plate with 370 MPa minimum yield, 510 MPa minimum tensile and Charpy V-notch impact of 120 J at −20°C for 12–100 mm plate. SHH STEEL supplies Q370qD mill-direct, TMCP / TMCP+T, up to 150 mm, with Z15–Z35, UT and heat and product analysis.
Keywords
Q370qD, Q370qD steel plate, GB/T 714 Q370qD, Q370q-D, Q370q D, Q370qD bridge steel, Q370qDZ15, Q370qDZ25, Q370qDZ35, bridge steel plate, Q370qD supplier
Equivalent Grades
No equivalent listed in Annex B / closest: EN 10025-4 S355ML–S420ML, ASTM A709 Grade 50 — Material Specification: GB/T 714-2025 (supersedes GB/T 714-2015) — Delivery: TMCP / TMCP+T (N >100 mm by agreement)
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q370q Quality Grades
GB/T 714-2025 vs 2015
Q370qD vs ASTM A709 / EN 10025
TMCP vs Normalized vs QT
Welding and Fatigue
Z15 / Z25 / Z35
Equivalent Material Grades
Testing and Inspection
Dimensions
Tolerances
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 714 Q370qD Bridge Steel Plate?

Q370qD is bridge structural steel plate to GB/T 714. Q stands for yield, 370 is the minimum yield in MPa for plate up to 50 mm, q stands for qiao (bridge) and D is the quality grade: Charpy V-notch at −20°C on longitudinal specimens.

Q370q is a step up from Q345q for railway and heavy highway bridges, where 25 MPa more yield trims plate thickness without changing chemistry or welding practice. Q370q uses the same TMCP chemistry box as Q345q (C ≤0.14%, CEV ≤0.38% to 50 mm), so a fabricator qualified on Q345q moves to Q370q with few changes. It is a favourite on heavy-haul and high-speed railway trusses.

Q370qD is the standard choice for railway truss bridges and heavy highway girders in central and northern China. It keeps Q345q chemistry and welding behaviour but adds 25 MPa yield and 20 MPa tensile, which shows up as thinner chords and fewer weld passes.

GB/T 714-2015 is no longer current. Its replacement, GB/T 714-2025, was published on 31 October 2025 and became effective on 1 May 2026. Where a contract still names the 2015 edition, we certify to it and flag any difference from 2025.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q370qD cut to size with an EN 10204 3.1 or 3.2 certificate. Sister grades are listed under GB/T 714.

Material Specification

Specification element Requirement SHH STEEL compliance
Standard GB/T 714-2025 Q370qD Confirmed
Product Single-rolled plate ≤150 mm; hot-rolled strip and cut plate ≤25.4 mm Plate
Thickness with tensile values Up to 150 mm for Q370q Confirmed
Minimum yield ReL 370 MPa ≤50 mm; 360 MPa >50–100 mm Confirmed
Minimum tensile Rm 510 MPa ≤100 mm (no upper limit in the standard) Confirmed
Elongation A ≥ 20% Confirmed
Charpy V-notch −20°C, 120 J (12–100 mm), longitudinal Confirmed
Delivery condition TMCP or TMCP + tempering; normalized by agreement for >100–150 mm As ordered
Weldability index CEV (Table 6) and Pcm (Table 7) Printed on MTC
Ultrasonic testing Plate >20 mm: GB/T 2970, Class II or better Every plate
Through-thickness Z15, Z25 or Z35 to GB/T 5313, when ordered As ordered
Dimensions GB/T 709 Confirmed
Certificate GB/T 247; EN 10204 3.1 or 3.2 As ordered

Grades often compared with Q370qD are ASTM A709 Grade 50, EN 10025-4 S355M and EN 10025-4 S420M; the comparison below shows where they differ.

Chemical Composition: Heat Analysis and Product Analysis

Bridge owners increasingly order a product analysis on finished plate. For Q370qD that check is judged against GB/T 714 heat limits plus the deviations in GB/T 222, not against the heat limits alone.

Table 1 below is the heat (ladle) analysis for Q370qD from GB/T 714-2025 Tables 1, 2 and 3.

Element Q370qD TMCP (%) Q370q normalized, >100–150 mm (%)
C, max 0.14 0.18
Si, max 0.55 0.55
Mn 0.80 – 1.60 1.00 – 1.60
P, max 0.025 0.025
S, max 0.015 0.015
Nb 0.010 – 0.090 0.005 – 0.060
V 0.010 – 0.080 0.010 – 0.080
Ti 0.006 – 0.030 0.006 – 0.030
Als 0.010 – 0.045 0.010 – 0.045
Cr, max 0.30 0.30
Ni, max 0.30 0.30
Cu, max 0.30 0.30
Mo, max — —
N, max 0.0080 0.0080
B, max 0.0005 residual (≤0.0014 if C ≤0.10%) 0.0005 residual
H, max 0.0002 0.0002

Nb, V, Ti and Al may be added singly or together. Added singly, each must meet the range above; added together, at least one must reach its minimum and Nb + V + Ti ≤ 0.22%.

Table 2 is the product analysis: the limits a check analysis on finished plate is judged against. GB/T 714-2025 clause 7.1.3 calls up GB/T 222 for the permitted deviations.

Element Heat limit (%) Deviation, GB/T 222-2025 Table 1 Q370qD product analysis (%)
C ≤ 0.14 +0.02 ≤ 0.16
Si ≤ 0.55 +0.05 ≤ 0.60
Mn 0.80 – 1.60 ±0.06 0.74 – 1.66
P ≤ 0.025 +0.005 ≤ 0.030
S ≤ 0.015 +0.005 ≤ 0.020
V 0.010 – 0.080 +0.02 / −0.01 ≤ 0.100
Ti 0.006 – 0.030 +0.02 / −0.01 ≤ 0.050
Nb 0.010 – 0.090 ±0.005 (listed for 0.015–0.060%) Above 0.060%: agree in contract
Cr ≤ 0.30 +0.05 ≤ 0.35
Ni ≤ 0.30 +0.05 ≤ 0.35
Cu ≤ 0.30 +0.05 ≤ 0.35
Als 0.010 – 0.045 ±0.003 Lower limit −0.003 (Table 1 row is for Al ≥0.015%; confirm)
Mo — Not listed in Table 1 —
N ≤ 0.0080 Listed only for 0.010–0.020% Agree in contract

How to read Table 2. Q370q TMCP heats are low-alloy steel, so Table 1 of GB/T 222 applies. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn falls in the 0.80–1.70% band, so ±0.06%. For one heat, an element may deviate in one direction only.

Mechanical Properties

Tensile values follow Table 9 of GB/T 714-2025 for Q370q. Tensile specimens are transverse; round specimens are used above 40 mm. Where yield is not distinct, Rp0.2 replaces ReL.

Nominal thickness ReL min (MPa) Rm min (MPa) A min
≤ 50 mm 370 510 20%
> 50 – 100 mm 360 510 20%
> 100 – 130 mm 320 430 20%
> 130 – 150 mm 320 430 20%

Impact values follow Table 10, on longitudinal specimens, average of three:

Letter / test temperature KV2 ≤12 mm KV2 >12 – 100 mm KV2 >100 – 150 mm
D / −20°C 80 J 120 J 47 J

One single value may fall below the required average, but not below 70% of it. Plate over 8 mm and under 12 mm is tested with 7.5 mm specimens (75% of the value); 6–8 mm plate with 5 mm specimens (50%). Plate under 6 mm is not impact tested.

180° bend test, transverse: mandrel D = 2a up to 16 mm and 3a above 16 mm; may be omitted when the mill guarantees it. Yield ratio is not mandatory. If the contract asks for it, Annex C recommends ReL/Rm ≤ 0.88 up to 12 mm and ≤ 0.85 above 12 mm for TMCP plate.

Q370qC / Q370qD / Q370qE: Which Quality Grade?

Q370qD is tested at −20°C. It suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C. D is the most specified letter on Chinese bridge drawings. It is tested at −20°C and the melt is tighter than C: P ≤0.025%, S ≤0.015%.

Grade Test temp. KV2 ≤12 mm KV2 12–100 mm KV2 >100 mm P / S max (%)
Q370qC 0°C 80 J 120 J 55 J 0.030 / 0.025
Q370qD −20°C 80 J 120 J 47 J 0.025 / 0.015
Q370qE −40°C 80 J 120 J 31 J 0.020 / 0.010

Over-specifying the letter costs money; under-specifying it costs safety. Choose from the lowest service or erection temperature, then step up one letter for thick, restrained or fracture-critical members.

Q370qD: What Changed from GB/T 714-2015 to GB/T 714-2025

For Q370qD buyers the 2025 edition changes more than the year on the certificate. The points below come from the foreword of GB/T 714-2025 and its tables.

  • Yield values above 100 mm were added (320 MPa for >100–130 mm).
  • The Mn range for TMCP steel was revised: the minimum is now 0.80%, and the maximum may be raised to 2.00% by agreement.
  • CEV and Pcm limits were revised (Tables 6 and 7).
  • Normalized grades were dropped except for plate over 100 mm by agreement.
  • Tensile strength is now banded by thickness (e.g. lower minimum Rm above 100 mm) instead of one value.
  • Impact energy is set by thickness band (≤12 mm, 12–100 mm, >100 mm) in Table 10.
  • Yield ratio is no longer a clause value; it is agreed in the contract, with recommendations in informative Annex C.
  • Section products were removed; the standard now covers plate and strip only.
  • Delivery is TMCP, TMCP + tempering or QT; normalizing is kept only for Q345q/Q370q plate over 100 mm by agreement.

If a drawing cites 2015 and the plate is made to 2025, get the designer’s written acceptance; tensile strength above 100 mm and the yield-ratio basis differ.

Q370qD vs ASTM A709 and EN 10025: Which Grade Matches?

Can Q370qD replace a US or European bridge grade, or the other way round? Strength can match; toughness rules differ in kind, not only in number.

Property Q370qD ASTM A709 Grade 50 EN 10025-4 S355M EN 10025-4 S420M
Min. yield (MPa) 370 (≤50 mm) 345 355 (≤16 mm) 420 (≤16 mm)
Tensile (MPa) 510 min 450 min 470 – 630 520 – 680
Charpy 120 J at −20°C (12–100 mm) CVN by temperature zone and member type (T / F) 40 J at −20°C 40 J at −20°C
Weathering chemistry No No No No

ASTM A709 sets Charpy requirements by temperature zone (1, 2, 3) and by member type: non-fracture-critical (T) or fracture-critical (F). GB/T 714 sets one value per letter, so compare the A709 zone with the GB/T 714 test temperature, not grade with grade.

EN 10025-3/-4/-6 grades show yield at the thinnest band; their values fall with thickness. GB/T 714 keeps 370 MPa to 50 mm. EN tensile ranges have upper limits; GB/T 714 gives minimums only.

The 120 J requirement in GB/T 714 for 12–100 mm plate is several times the 27–40 J typical of general structural grades. That margin is the main reason bridge owners specify Q370qD rather than GB/T 1591 plate.

Q370qD Delivery Condition: TMCP vs Normalized vs Quenched and Tempered

GB/T 714-2025 clause 3.2 defines TMCP as rolling with the final deformation in a controlled temperature range, including accelerated cooling with or without tempering (self-tempering included) but excluding direct quenching and quench-and-temper. The delivery route must be stated on the certificate.

Route Available for Q370qD Weldability index Notes
TMCP Yes, standard CEV (C >0.12%) or Pcm (C ≤0.12%) C ≤0.14%; most plate up to 100 mm
TMCP + tempering Yes Same as TMCP Used to relieve stresses or tune yield ratio
Normalized Only >100–150 mm, by agreement CEV by agreement C ≤0.18%; heavy plate only
Quenched and tempered Not listed — Not a GB/T 714 route at this level

Q370q follows the same pattern as Q345q: TMCP as standard, normalized only for plate over 100 mm by agreement. D-letter plate is usually plain TMCP; tempering is added mainly for heavy plate or tight yield-ratio limits.

Ask for the route on the purchase order. It changes the weldability index, the welding procedure and, for heavy plate, the price of Q370qD.

Welding Q370qD and Fatigue in Bridge Girders

GB/T 714-2025 clause 7.1.2 uses CEV for normalized, QT and TMCP steel with C >0.12%, and Pcm for weathering steel and TMCP steel with C ≤0.12%, both from the heat analysis:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Index ≤50 mm >50–100 mm >100–130 mm
CEV, TMCP, C >0.12% (Table 6) ≤ 0.38 ≤ 0.40 by agreement
Pcm, TMCP (Table 7) ≤ 0.20 ≤ 0.20 ≤ 0.20
CEV, normalized — — By agreement

For Q370qD, ask the fabricator which index the WPS was qualified on. Where the WPS uses CEV and the standard uses Pcm, we print both on the certificate. At −20°C, most procedures qualified on TMCP plate pass HAZ impact without special measures; keep multi-wire SAW heat input inside the qualified band.

Typical consumables for Q370qD: E50/E55-class low-hydrogen consumables (AWS E7018 / E8018 type).

Fatigue. Welded details govern fatigue life in a bridge, and their fatigue strength is set by detail category, not by yield strength. Higher-strength plate can carry higher stress ranges only if detailing improves too.

Fatigue design follows JTG D64 (highway) and TB 10091 (railway) in China, EN 1993-1-9 in Europe and AASHTO LRFD in the US; fabrication commonly follows TB 10212, JTG/T 3650 or AWS D1.5.

Q370qDZ15, Z25 and Z35: Through-Thickness Plate for Bridges

On long-span bridges, Z25 or Z35 is common on node plates and anchor zones. The extra cost is in desulfurization, testing and a higher reject rate.

GB/T 714 adds the Z level to the end of the designation, for example Q370qDZ25. The test and acceptance follow GB/T 5313 and apply to plate 15 mm and thicker.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

D chemistry allows S up to 0.015%. Z15 needs S ≤0.010% and Z25 needs ≤0.007%, so Z plate is still made from a dedicated low-sulfur heat.

Ask your designer which Q370qD plates are loaded through the thickness. Ordering Z35 on everything costs money and time without adding safety. Z options apply across the GB/T 714 bridge steel range.

Equivalent Material Grades

Annex B of GB/T 714-2025 lists foreign grades against each strength level. It is informative: it tells you which families are close, not that the plates are interchangeable.

Standard Grade(s) Fit for Q370qD
ASTM A709 ASTM A709 Grade 50 Closest; lower yield
EN 10025-4 EN 10025-4 S355ML, EN 10025-4 S420M Bracketing grades
GB/T 1591 GB/T 1591 Q390MD General structural, higher yield, lower impact
JIS G3106 JIS G3106 SM520C Closest by strength
GB/T 714 (weathering twin) Q370qNHD Same strength, weathering chemistry

Before substituting, compare three things line by line: minimum yield at the actual thickness, the impact test temperature and energy, and the weldability index. For Q370qD, the 120 J impact level and the Pcm/CEV caps are usually the hardest to match.

Q370qD Testing, UT and Certificate

A batch of Q370qD is one grade, one heat, one thickness, one rolling schedule and one heat-treatment condition, up to 60 t. Table 12 of GB/T 714-2025 sets the tests:

Test Frequency Method
Heat analysis 1 per heat GB/T 20066; GB/T 4336 / GB/T 223
Tensile 1 per batch GB/T 2975 / GB/T 228.1
Bend 180° 1 per batch (may be waived if guaranteed) GB/T 232
Charpy V at −20°C 3 specimens per batch GB/T 229
Through-thickness (Z) 3 specimens per batch, when ordered GB/T 5313
Ultrasonic Every plate >20 mm, Class II or better GB/T 2970
Surface and dimensions Every plate Visual and gauges

Impact retest: if a set fails, three more specimens are taken from the same batch. The average of all six must meet the requirement; two values may be below it, but only one below 70%. At −20°C the 120 J level is comfortable for well-made TMCP plate, but we still check each batch value, not just the average.

Dimensions

Size range for Q370qD plate:

  • Thickness: 6 mm – 150 mm under GB/T 714 tensile tables; most orders 8 – 60 mm
  • Width: 1500 – 4000 mm, depending on mill and thickness
  • Length: 6000 – 18000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, 7.85 g/cm³

Deck plate, webs, flanges, diaphragms and stiffeners are cut to drawing. For U-ribs and rolled sections on the same bridge, see steel beam profiles and steel structural profiles.

Tolerances

Q370qD plate is rolled to GB/T 709 tolerances. Class B (−0.30 mm) is standard; Class C (zero minus) can be agreed.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Bridge fabricators often ask for Class C (zero minus) on deck and flange plate so section properties are never under the design value. Wider plates follow the heavier GB/T 709 rows; we state them on the offer.

Q370qD Price Factors and How to Order

Bridge plate prices move with the steel market, but for Q370qD the order details often matter more.

Cost driver Effect on price
Strength level Q370q Higher levels need more alloy and tighter rolling control
Quality letter Small extra for −20°C testing and cleaner melt
Delivery route TMCP / TMCP+T (N >100 mm by agreement)
Thickness Over 60 mm and under 10 mm carry size extras
Z15 / Z25 / Z35 Low-sulfur heat, Z test, UT; Z35 costs most
Width and length Over 3000 mm wide or 15 m long needs mill confirmation
Quantity per size Mill minimums per heat and size
Inspection and processing 3.2 witness, profile cutting, blasting, priming quoted per item

To get a firm quote in one round, send:

  • Grade, edition and Z level, e.g. Q370qDZ25 to GB/T 714-2025
  • Thickness × width × length and pieces or tonnes
  • Delivery route and UT class if beyond Class II
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line. Need another letter? See Q370qC, Q370qE.

Applications

Sector Typical Q370qD components
Railway trusses Chords, diagonals and node plates on steel truss bridges
High-speed rail Box girders and plate girders on long-span crossings
Highway bridges Main girders where Q345q thickness becomes awkward to weld
Combined road-rail bridges Truss members and deck system
Arch bridges Arch ribs and tie girders

The letter D suits most highway and railway bridges in central and northern China, Europe and North America, where winter lows reach about −20°C.

It is the wrong plate for pressure equipment (pressure vessel steel plates), unpainted exposure (weathering steel plates) or ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q370qD from first-line bridge-plate mills, including drafters of GB/T 714-2025 such as Ansteel, Valin Xiangtan, Jiangyin Xingcheng, Wuyang, Shougang and Xinyu.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness (SGS, BV, TÜV or owner’s inspector)
  • Tests: tensile, −20°C Charpy, bend, Z test, UT, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blasting and priming
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill, per GB/T 247

We ship Q370qD to fabricators in Asia, Africa, the Middle East, Europe and the Americas, by break-bulk or container.

Lead time: about 30–45 days from mill rolling; Z35, F letter or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Southeast Asia and 28–35 days to North Europe.

Why Choose SHH STEEL

SHH STEEL is a steel manufacturer and exporter and global steel mill sourcing partner. We buy Q370qD mill-direct, China origin, and check every certificate before shipment.

Before shipment we check four lines on every Q370qD certificate: yield and tensile for the actual thickness band, Charpy at −20°C, the CEV or Pcm for the delivery route, and UT results. If one fails, the plate does not ship as Q370qD.

On mixed Q345qD/Q370qD projects, ask us to mark the grades in different paint colours. Mix-ups on site are the most common quality incident we see on such jobs.

We also tell buyers when another grade fits better. Neighbouring levels are Q345qD and Q390q. The weathering counterpart is Q370qNHD. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q370qD steel?
Q370qD is bridge structural steel plate to GB/T 714-2025. It has 370 MPa minimum yield up to 50 mm, 510 MPa minimum tensile, 20% elongation and Charpy V-notch impact of 120 J at −20°C for 12–100 mm plate. It is delivered TMCP or TMCP + tempering, with normalizing allowed above 100 mm by agreement.
What is the difference between Q370qD and Q370qE?
Strength and chemistry box are the same. Q370qD is Charpy tested at −20°C, Q370qE at −40°C, both needing 120 J for 12–100 mm plate. P/S caps are 0.025/0.015% for D and 0.020/0.010% for E. Choose by the lowest service or erection temperature.
What is the maximum thickness of Q370qD?
150 mm. GB/T 714-2025 covers single-rolled bridge plate up to 150 mm and gives Q370q tensile values for every band to 150 mm: 370 MPa yield to 50 mm, 360 MPa to 100 mm and 320 MPa above. Plate over 100 mm may be normalized by agreement.
What is the ASTM or EN equivalent of Q370qD?
Close grades for Q370qD: No equivalent listed in Annex B / closest: EN 10025-4 S355ML–S420ML, ASTM A709 Grade 50. These are close families, not drop-in substitutes; compare yield at thickness, impact temperature and energy, and the weldability index before substituting.
How is Q370qD marked?
Plates are marked per GB/T 247 with grade, heat number, size and mill, and the Z level if ordered, for example Q370qDZ25. The certificate must state the delivery condition (TMCP, TMCP + tempering or QT).
Is Q370qD weldable?
Yes. GB/T 714-2025 caps the weldability index for Q370qD up to 50 mm at CEV ≤0.38% (C >0.12%) or Pcm ≤0.20%. Preheat depends on actual chemistry, thickness and restraint, and is fixed by the qualified welding procedure.

Conclusion

Q370qD to GB/T 714-2025 is bridge plate with 370 MPa minimum yield, 510 MPa minimum tensile and 120 J Charpy at −20°C for 12–100 mm plate.

It sits between Q345qD and Q390q in the bridge range, with Q370qC and Q370qE as sister letters. The most common ordering mistake with Q370qD is leaving the Z level, UT class or impact position off the order; add them at enquiry stage, not after rolling.

From SHH STEEL, Q370qD arrives with traceable heat numbers, a complete EN 10204 3.1 or 3.2 certificate and, if ordered, third-party witness, product analysis and Z testing.

We ship from Shanghai to bridge builders worldwide. Browse the full GB/T 714 range or other high strength low alloy plates.

Email the cutting list and the owner’s specification. We return a line-by-line offer with test plan and lead time. Contact SHH STEEL for Q370qD bridge steel plate.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X