GB/T 3531 15MnNiDR Steel Plate | 15MnNiDR -45°C Vessel Plate | GB/T 3531 Steel - SHH STEEL

GB/T 3531 15MnNiDR Steel Plate | 15MnNiDR -45°C Vessel Plate

GB/T 3531 15MnNiDR is manganese-nickel steel plate for low-temperature pressure vessels under GB/T 3531-2014. It is supplied normalized or normalized and tempered in 6–60 mm, with Charpy V-notch energy of 60 J minimum at -45°C. The grade was dropped from the 2023 successor standard, so it is now ordered to the 2014 edition or to a project specification that names it. SHH STEEL produces and exports 15MnNiDR plate when the project documents call for it.
Equivalent Grades:
Near: EN 10028-4 13MnNi6-3, EN 10028-3 P355NL2. No GB/T 713.3-2023 successor exists. None is automatic.
Heat Treatment
Normalized, or normalized and tempered (GB/T 3531-2014 Table 2).
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is GB/T 3531-2014 15MnNiDR steel plate?

GB/T 3531 15MnNiDR Steel Plate is a manganese-nickel, aluminium-killed plate for welded pressure vessels in low-temperature service, ordered to GB/T 3531-2014. A nickel addition of 0.20–0.60 % and a small vanadium allowance raise strength and toughness above 16MnDR, and the impact test is at -45°C.

GB/T 3531-2014, Steel plates for low temperature pressure vessels, was issued on 24 June 2014 as GB 3531-2014 and implemented on 1 April 2015, replacing GB 3531-2008. It was later converted to a recommended national standard, which is why it is cited as GB/T 3531-2014. It covers plates 5 mm to 120 mm thick for pressure vessels working from -196°C to below -20°C. The edition was withdrawn on 1 March 2024 and replaced by GB/T 713.3-2023, with the nickel grades moved to GB/T 713.4-2023.

15MnNiDR is not in GB/T 713.3-2023. The 2023 book deleted 15MnNiDR from its grade list, so there is no GB/T 713.3 15MnNiDR product and no successor page for it on this site. Where 15MnNiDR is still named on a drawing, data sheet or replacement order, it is supplied to GB/T 3531-2014. Designers moving to the 2023 book re-select a grade by design temperature, for example GB/T 713.3 13MnNiDR or GB/T 713.3 09MnNiDR; that is a design decision, not a one-for-one replacement.

SHH STEEL produces and exports GB/T 3531-2014 15MnNiDR plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry. This grade is listed in our GB/T 3531 range under Nuclear-Grade Steel Plates.

Material specification for GB/T 3531 15MnNiDR

The items below follow GB/T 3531-2014. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard GB/T 3531-2014, Steel plates for low temperature pressure vessels (issued as GB 3531-2014; replaced GB 3531-2008)
Edition status Withdrawn 1 March 2024. Replaced by GB/T 713.3-2023 for the low-alloy grades and GB/T 713.4-2023 for 08Ni3DR and 06Ni9DR. This page covers the 2014 edition only
Scope of the standard Plates 5 mm to 120 mm thick for low-temperature pressure vessels from -196°C to below -20°C
Grades in the 2014 edition 16MnDR, 15MnNiDR, 15MnNiNbDR, 09MnNiDR, 08Ni3DR, 06Ni9DR
Grade 15MnNiDR
Delivery condition (Table 2) Normalized, or normalized and tempered
Impact requirement -45°C / 60 J for all tabulated thicknesses
2023 status Deleted from GB/T 713.3-2023; no successor designation
Thickness tabulated for this grade 6–60 mm (standard limits in Table 2, not a stock range)
Steelmaking Basic oxygen or electric furnace with secondary refining. Reduction ratio at least 3 from continuous-cast slab or ingot, at least 2 from electroslag remelted slab
Dimensions and tolerances GB/T 709-2006, thickness tolerance Class B; Class C or tighter tolerances by agreement
Ultrasonic testing Plate by plate for N or N+T plate over 20 mm and Q+T plate over 16 mm; method JB/T 4730.3, GB/T 2970 or GB/T 28297, class stated on the contract
Our supply We produce and export 15MnNiDR plate to GB/T 3531-2014 with the dimensions, tests and inspection document written on the enquiry

Chemical composition of GB/T 3531-2014 15MnNiDR

The heat analysis below is the 15MnNiDR row of GB/T 3531-2014 Table 1. Sulfur is held to 0.008 % maximum, tighter than for 16MnDR.

Element Heat analysis, GB/T 3531-2014 Table 1 (wt. %)
Carbon (C) ≤0.18
Silicon (Si) 0.15–0.50
Manganese (Mn) 1.20–1.60
Nickel (Ni) 0.20–0.60
Vanadium (V) ≤0.05
Total aluminium (Alt) ≥0.020
Phosphorus (P) ≤0.020
Sulfur (S) ≤0.008

Notes to Table 1: Als may be determined instead of Alt, in which case Als shall be not less than 0.015 %; when Nb + V + Ti exceeds 0.015 %, aluminium is not an acceptance requirement. Nb, V and Ti may be added to improve properties, with Nb + V + Ti not more than 0.12 %, and the amounts added reported on the certificate. As residual elements, Cr and Cu are each limited to 0.25 % and Mo to 0.08 %, and Ni to 0.40 % where nickel is not a specified alloying element; the supplier need not analyse them when it guarantees compliance. Product analysis tolerances follow GB/T 222.

Mechanical properties of GB/T 3531-2014 15MnNiDR

Table 2 of GB/T 3531-2014 tabulates 15MnNiDR in three thickness bands up to 60 mm. The impact requirement is the same -45°C / 60 J across all bands.

Nominal thickness (mm) Tensile strength Rm (MPa) Yield strength ReL, min (MPa) Elongation A, min (%) Charpy V test temperature KV2, min (J) 180° bend, b = 2a
6–16 490–620 325 20 -45°C 60 D = 3a
>16–36 480–610 315 20 -45°C 60 D = 3a
>36–60 470–600 305 20 -45°C 60 D = 3a

Charpy V-notch energy is the mean of three specimens. One single value may fall below the Table 2 figure, but not below 70 % of it. Plates under 12 mm are tested with sub-size specimens: 10 × 7.5 × 55 mm for plate over 8 mm and under 12 mm, with results not less than 75 % of the Table 2 value, and 10 × 5 × 55 mm for 6–8 mm plate, with results not less than 50 %. Plate thinner than 6 mm is not impact tested. Higher impact energy than Table 2 may be agreed and written on the contract. Yield is ReL; where yielding is not distinct, Rp0.2 is measured instead. In the bend column, a is the specimen thickness and D the mandrel diameter; the bend test may be waived when the supplier guarantees it.

Delivery conditions for GB/T 3531 15MnNiDR

Table 2 lists 15MnNiDR as normalized, or normalized and tempered. State the condition on the order, or accept either. If the vessel will be post-weld heat treated, ask for simulated PWHT testing so toughness is proved after the thermal cycle.

Because the 2023 book no longer covers this grade, the order must name GB/T 3531-2014 explicitly. A certificate to GB/T 713.3-2023 cannot list 15MnNiDR.

Welding and thermal cutting

Nickel improves heat-affected-zone toughness, and the low sulfur level helps through-thickness properties. Weld metal must reach the -45°C impact requirement, which usually means nickel-bearing low-temperature consumables chosen by the qualified procedure.

Preheat, heat input, interpass temperature and post-weld heat treatment are set by the procedure qualification, the thickness and the vessel code.

Dimensions, tolerances and inspection

Dimensions, shape and permitted deviations follow GB/T 709-2006. Thickness tolerance is Class B unless the purchaser asks for Class C, and tighter tolerances may be agreed. Plates are invoiced on theoretical weight, calculated from the mean of the maximum and minimum permitted thickness.

Cracks, blisters, scabs, folds and inclusions are not permitted on the surface. They may be removed by dressing, provided the dressed depth does not exceed half the thickness tolerance and the minimum permitted thickness is kept. Dressed areas must be smooth.

Acceptance is by batch: one grade, one heat, one thickness and one heat-treatment condition, not more than 30 t per batch; a single plate heavier than 30 t is its own batch. Each batch receives one tensile test, one bend test and a set of three Charpy specimens; chemical analysis is one per heat. Ultrasonic testing is plate by plate for normalized or normalized-and-tempered plate thicker than 20 mm.

Applications and specification limits

We produce and export 15MnNiDR for low-temperature vessels, spherical tanks and heat exchangers designed around a -45°C impact class, typically in LPG, propylene and other refrigerated process service. The allowable minimum design temperature is set by the vessel code and the impact test, not by the grade name.

Table 2 covers 15MnNiDR only up to 60 mm. Thicker plate is outside the tabulated range and would need its own written agreement.

Edition note. This page is the GB/T 3531-2014 product. Unlike 16MnDR, 09MnNiDR and 15MnNiNbDR, this grade has no GB/T 713.3-2023 successor: 15MnNiDR was removed from that list. The 2014 and 2023 books are not the same specification, and a certificate to one edition is not an automatic substitute for an order written to the other.

GB/T 3531-2014 is a low-temperature pressure vessel plate standard. On its own it does not impose nuclear-class requirements; where a nuclear or other special code applies, its supplementary requirements must be written on the order.

Compare GB/T 3531 15MnNiDR with other low-temperature plates

The comparison below places 15MnNiDR between 16MnDR and 15MnNiNbDR in the 2014 book, and against a 2023 Mn-Ni grade that designers consider instead. These are related grades, not interchangeable ones.

Material Type Delivery Key requirement Substitution limit
GB/T 3531 15MnNiDR (this plate) Mn-Ni, Al-killed N or N+T ReL 325 MPa min at 6–16 mm; -45°C / 60 J; to 60 mm 2014 edition only; no 2023 successor
GB/T 3531 16MnDR C-Mn N or N+T ReL 315 MPa min at 6–16 mm; -40°C / 47 J to 60 mm Higher test temperature, lower energy
GB/T 3531 15MnNiNbDR Mn-Ni-Nb N or N+T ReL 370 MPa min at 10–16 mm; -50°C / 60 J Higher strength; different design allowables
GB/T 3531 09MnNiDR Low-C Mn-Ni N or N+T ReL 300 MPa min at 6–16 mm; -70°C / 60 J Lower strength, deeper cold
GB/T 713.3 13MnNiDR Mn-Ni (2023 edition) See that page 2023 tables; see that page A 2023 grade, not a renamed 15MnNiDR

Equivalent and related grades by country

The grades below are near equivalents by chemistry family or impact class, not certified equivalents. Check strength bands, impact temperature and thickness limits against the project specification.

Country / region Standard Grade Similarity and key differences Caveat
China GB/T 3531-2014 15MnNiDR This product —
China GB/T 713.3-2023 None 15MnNiDR was deleted from the 2023 list No successor designation
Europe EN 10028-4 EN 10028-4 13MnNi6-3 Normalized Mn-Ni plate for low-temperature vessels Different nickel window and impact rules
Europe EN 10028-3 EN 10028-3 P355NL2 Normalized fine-grain C-Mn plate in a lower impact temperature class No nickel requirement
United States ASTM A537 ASTM A537 Class 1 Normalized C-Mn-Si vessel plate Impact only by supplementary requirement
Japan JIS G3126 JIS G3126 SLA325B Low-temperature C-Mn vessel plate Different impact temperature and strength class

Why choose SHH STEEL for GB/T 3531 15MnNiDR

  • SHH STEEL produces and exports GB/T 3531-2014 15MnNiDR plate as a producer, exporter and mill agent
  • We quote to the edition written on your order and keep GB/T 3531-2014 values separate from GB/T 713.3 or GB/T 713.4 values
  • We quote 15MnNiDR to GB/T 3531-2014 by name, because the 2023 book no longer lists it
  • We review impact temperature, ultrasonic class and any simulated PWHT before quoting, not after rolling
  • We match the inspection document to what the purchase order requires

How to enquire for GB/T 3531 15MnNiDR plate

Item What to specify
Standard and grade GB/T 3531-2014 15MnNiDR; state the edition year rather than only GB/T 3531
Delivery condition Normalized, or normalized and tempered; state if simulated PWHT is required
Dimensions Thickness, width and length; we confirm production and export feasibility against the enquiry
Impact testing Table 2 temperature and energy, or a higher agreed energy; state specimen orientation if the project specifies it
Ultrasonic testing JB/T 4730.3, GB/T 2970 or GB/T 28297, with the acceptance class
Supplementary tests Simulated post-weld heat treatment, through-thickness or product analysis only when written on the order
Documentation Inspection document type required by the project, for example EN 10204 3.1 or 3.2
Other editions If GB/T 713.3-2023 or GB/T 713.4-2023 must also be met, say so on the enquiry; we review both editions before quoting

FAQ

Is 15MnNiDR in GB/T 713.3-2023?
No. GB/T 713.3-2023 deleted 15MnNiDR from its grade list. The grade is ordered to GB/T 3531-2014 or to a project specification that names it.
What replaces 15MnNiDR in the 2023 standard?
There is no direct replacement. Designers re-select a GB/T 713.3-2023 grade by design temperature and strength, for example 13MnNiDR or 09MnNiDR, with the change approved under the vessel code.
What are the impact requirements for 15MnNiDR?
GB/T 3531-2014 Table 2 requires 60 J minimum at -45°C for all tabulated thicknesses from 6 mm to 60 mm.
What thickness does GB/T 3531-2014 cover for 15MnNiDR?
Table 2 tabulates 6–16 mm, over 16–36 mm and over 36–60 mm. These are standard limits, not a stock range.
What should a quotation enquiry include?
GB/T 3531-2014, grade 15MnNiDR, delivery condition, thickness by width by length, quantity, impact and ultrasonic requirements, any simulated PWHT, and the inspection document.

Request a quotation

Contact SHH STEEL for a quotation for GB/T 3531-2014 15MnNiDR low-temperature pressure vessel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

State the delivery condition, the Charpy test temperature and energy if they differ from Table 2, the ultrasonic testing standard and class, any simulated post-weld heat treatment, and the inspection document required by the project.

If your project is moving to GB/T 713.3-2023 and needs a replacement grade, send the design temperature, thickness and vessel code. We will review the candidate grades rather than assume one replaces 15MnNiDR.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response