GB/T 3531 08Ni3DR Steel Plate | 08Ni3DR -100°C Vessel Plate | GB/T 3531 Steel - SHH STEEL

GB/T 3531 08Ni3DR Steel Plate | 08Ni3DR -100°C Vessel Plate

GB/T 3531 08Ni3DR is 3.5 % nickel steel plate for low-temperature pressure vessels under GB/T 3531-2014. It is supplied normalized, normalized and tempered, or quenched and tempered in 6–100 mm, with Charpy V-notch energy of 60 J minimum at -100°C. The grade moved to GB/T 713.4-2023 in the 2023 revision. SHH STEEL produces and exports 08Ni3DR plate to the 2014 edition when the project documents call for it.
Equivalent Grades:
Near: ASTM A203 Grade D / E, EN 10028-4 12Ni14, JIS G3127 SL3N255 / SL3N275. Successor: GB/T 713.4 08Ni3DR. None is automatic.
Heat Treatment
Normalized, N+T or Q+T; tempering not below 600°C; over 60 mm N + accelerated cooling + T by agreement.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is GB/T 3531-2014 08Ni3DR steel plate?

GB/T 3531 08Ni3DR Steel Plate is a 3.5 % nickel steel plate (Ni 3.25–3.70 %) for welded pressure vessels in deep low-temperature service, ordered to GB/T 3531-2014. It was one of the three grades added in the 2014 edition, and its impact test is at -100°C.

GB/T 3531-2014, Steel plates for low temperature pressure vessels, was issued on 24 June 2014 as GB 3531-2014 and implemented on 1 April 2015, replacing GB 3531-2008. It was later converted to a recommended national standard, which is why it is cited as GB/T 3531-2014. It covers plates 5 mm to 120 mm thick for pressure vessels working from -196°C to below -20°C. The edition was withdrawn on 1 March 2024 and replaced by GB/T 713.3-2023, with the nickel grades moved to GB/T 713.4-2023.

In the 2023 revision this designation moved out of the low-alloy book into the nickel-steel book, as GB/T 713.4 08Ni3DR. Order this page when the drawing or data sheet still names GB/T 3531-2014.

SHH STEEL produces and exports GB/T 3531-2014 08Ni3DR plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry. This grade is listed in our GB/T 3531 range under Nuclear-Grade Steel Plates.

Material specification for GB/T 3531 08Ni3DR

The items below follow GB/T 3531-2014. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard GB/T 3531-2014, Steel plates for low temperature pressure vessels (issued as GB 3531-2014; replaced GB 3531-2008)
Edition status Withdrawn 1 March 2024. Replaced by GB/T 713.3-2023 for the low-alloy grades and GB/T 713.4-2023 for 08Ni3DR and 06Ni9DR. This page covers the 2014 edition only
Scope of the standard Plates 5 mm to 120 mm thick for low-temperature pressure vessels from -196°C to below -20°C
Grades in the 2014 edition 16MnDR, 15MnNiDR, 15MnNiNbDR, 09MnNiDR, 08Ni3DR, 06Ni9DR
Grade 08Ni3DR
Delivery condition (Table 2) Normalized, normalized and tempered, or quenched and tempered
Impact requirement -100°C / 60 J for all tabulated thicknesses
Tempering Not lower than 600°C
Mechanical test frequency Each heat-treated plate when delivered N+T or Q+T
Thickness tabulated for this grade 6–100 mm (standard limits in Table 2, not a stock range)
Steelmaking Basic oxygen or electric furnace with secondary refining. Reduction ratio at least 3 from continuous-cast slab or ingot, at least 2 from electroslag remelted slab
Dimensions and tolerances GB/T 709-2006, thickness tolerance Class B; Class C or tighter tolerances by agreement
Ultrasonic testing Plate by plate for N or N+T plate over 20 mm and Q+T plate over 16 mm; method JB/T 4730.3, GB/T 2970 or GB/T 28297, class stated on the contract
Our supply We produce and export 08Ni3DR plate to GB/T 3531-2014 with the dimensions, tests and inspection document written on the enquiry

Chemical composition of GB/T 3531-2014 08Ni3DR

The heat analysis below is the 08Ni3DR row of GB/T 3531-2014 Table 1. Phosphorus and sulfur limits are tighter than for the low-alloy grades.

Element Heat analysis, GB/T 3531-2014 Table 1 (wt. %)
Carbon (C) ≤0.10
Silicon (Si) 0.15–0.35
Manganese (Mn) 0.30–0.80
Nickel (Ni) 3.25–3.70
Vanadium (V) ≤0.05
Molybdenum (Mo) ≤0.12
Phosphorus (P) ≤0.015
Sulfur (S) ≤0.005

Notes to Table 1: as residual elements, Cr and Cu are each limited to 0.25 %; the supplier need not analyse them when it guarantees compliance. Product analysis tolerances follow GB/T 222, except that for 08Ni3DR and 06Ni9DR the permitted product-analysis excess is +0.003 % for phosphorus and +0.002 % for sulfur. Confirm residual limits on the mill test certificate.

Mechanical properties of GB/T 3531-2014 08Ni3DR

Table 2 of GB/T 3531-2014 tabulates 08Ni3DR in two bands up to 100 mm. The impact requirement is -100°C / 60 J in both.

Nominal thickness (mm) Tensile strength Rm (MPa) Yield strength ReL, min (MPa) Elongation A, min (%) Charpy V test temperature KV2, min (J) 180° bend, b = 2a
6–60 490–620 320 21 -100°C 60 D = 3a
>60–100 480–610 300 21 -100°C 60 D = 3a

Charpy V-notch energy is the mean of three specimens. One single value may fall below the Table 2 figure, but not below 70 % of it. Plates under 12 mm are tested with sub-size specimens: 10 × 7.5 × 55 mm for plate over 8 mm and under 12 mm, with results not less than 75 % of the Table 2 value, and 10 × 5 × 55 mm for 6–8 mm plate, with results not less than 50 %. Plate thinner than 6 mm is not impact tested. Higher impact energy than Table 2 may be agreed and written on the contract. Yield is ReL; where yielding is not distinct, Rp0.2 is measured instead. In the bend column, a is the specimen thickness and D the mandrel diameter; the bend test may be waived when the supplier guarantees it.

Delivery conditions for GB/T 3531 08Ni3DR

Table 2 lists 08Ni3DR as normalized, normalized and tempered, or quenched and tempered. When tempered, the tempering temperature shall be not lower than 600°C. With the purchaser’s agreement, plate thicker than 60 mm may be supplied normalized, accelerated cooled and tempered.

Normalized, N+T and Q+T plate are not interchangeable supply states; state the condition on the order. Plate delivered N+T or Q+T is mechanically tested plate by plate as heat treated.

Welding and thermal cutting

3.5 % nickel steel is welded with consumables qualified for -100°C toughness; nickel-alloy or matching nickel-steel consumables are chosen by the procedure. Heat input is controlled to protect heat-affected-zone toughness.

Nickel steels can pick up residual magnetism, which causes arc blow; check and demagnetise where necessary. Preheat, interpass temperature and post-weld heat treatment are set by the qualified procedure, the thickness and the vessel code.

Dimensions, tolerances and inspection

Dimensions, shape and permitted deviations follow GB/T 709-2006. Thickness tolerance is Class B unless the purchaser asks for Class C, and tighter tolerances may be agreed. Plates are invoiced on theoretical weight, calculated from the mean of the maximum and minimum permitted thickness.

Cracks, blisters, scabs, folds and inclusions are not permitted on the surface. They may be removed by dressing, provided the dressed depth does not exceed half the thickness tolerance and the minimum permitted thickness is kept. Dressed areas must be smooth.

Acceptance is by batch: one grade, one heat, one thickness and one heat-treatment condition, not more than 30 t per batch; a single plate heavier than 30 t is its own batch. Each batch receives one tensile test, one bend test and a set of three Charpy specimens; chemical analysis is one per heat. Plate delivered N+T or Q+T is mechanically tested per heat-treated plate. Ultrasonic testing is plate by plate for normalized or N+T plate over 20 mm and for Q+T plate over 16 mm.

Applications and specification limits

We produce and export 08Ni3DR for vessels and storage designed around a -100°C impact class, such as ethylene, ethane and propane low-temperature equipment and carbon dioxide liquefaction. The allowable minimum design temperature is set by the vessel code and the impact test. For LNG and liquid-nitrogen temperatures, a 9 % nickel grade such as GB/T 3531 06Ni9DR is used instead.

Edition note. This page is the GB/T 3531-2014 product. Its 2023 successor coverage is GB/T 713.4 08Ni3DR in GB/T 713.4-2023, the separate nickel-steel book. The 2014 and 2023 books are not the same specification, and a certificate to one edition is not an automatic substitute for an order written to the other.

GB/T 3531-2014 is a low-temperature pressure vessel plate standard. On its own it does not impose nuclear-class requirements; where a nuclear or other special code applies, its supplementary requirements must be written on the order.

Compare GB/T 3531 08Ni3DR with other low-temperature plates

The comparison below places 08Ni3DR against the 2014 grades on either side of it, its 2023 successor and other nickel steels. These grades are related, not interchangeable.

Material Type Delivery Key requirement Substitution limit
GB/T 3531 08Ni3DR (this plate) 3.5 % Ni N, N+T or Q+T ReL 320 MPa min at 6–60 mm; -100°C / 60 J; to 100 mm 2014 edition only
GB/T 3531 09MnNiDR Low-C Mn-Ni N or N+T -70°C / 60 J Not for -100°C service
GB/T 3531 06Ni9DR 9 % Ni Q+T -196°C / 100 J Deeper cold; different design
GB/T 713.4 08Ni3DR 3.5 % Ni (2023 edition) See that page 2023 tables; see that page Successor coverage, not the same specification
GB/T 713.4 07Ni5DR 5 % Ni (2023 edition) See that page 2023 tables New 2023 grade, not in GB/T 3531-2014
ASTM A203 Grade E 3.5 % Ni ASTM plate Per ASTM A203 Per ASTM A203 Different strength and impact rules

Equivalent and related grades by country

The grades below are near equivalents in the 3.5 % nickel family, not certified equivalents. Check strength bands, heat treatment and impact rules against the project specification.

Country / region Standard Grade Similarity and key differences Caveat
China GB/T 3531-2014 08Ni3DR This product —
China GB/T 713.4-2023 GB/T 713.4 08Ni3DR Same designation in the 2023 nickel-steel book Different edition; not automatic
United States ASTM A203 / ASME SA203 ASTM A203 Grade D, ASTM A203 Grade E, ASME SA203 Grade D, ASME SA203 Grade E 3.5 % nickel plate; Grade D lower and Grade E higher strength Impact test temperature and values differ
Europe EN 10028-4 EN 10028-4 12Ni14 3.5 % nickel plate for low-temperature vessels Different heat-treatment and impact rules
Japan JIS G3127 JIS G3127 SL3N255, JIS G3127 SL3N275 3.5 % nickel low-temperature plate Different strength classes

Why choose SHH STEEL for GB/T 3531 08Ni3DR

  • SHH STEEL produces and exports GB/T 3531-2014 08Ni3DR plate as a producer, exporter and mill agent
  • We quote to the edition written on your order and keep GB/T 3531-2014 values separate from GB/T 713.3 or GB/T 713.4 values
  • We state whether the plate is N, N+T or Q+T on the quotation, because GB/T 3531-2014 allows all three
  • We review impact temperature, ultrasonic class and any simulated PWHT before quoting, not after rolling
  • We match the inspection document to what the purchase order requires

How to enquire for GB/T 3531 08Ni3DR plate

Item What to specify
Standard and grade GB/T 3531-2014 08Ni3DR; state the edition year rather than only GB/T 3531
Delivery condition Normalized, normalized and tempered, or quenched and tempered; over 60 mm, normalized + accelerated cooling + tempered if agreed
Dimensions Thickness, width and length; we confirm production and export feasibility against the enquiry
Impact testing Table 2 temperature and energy, or a higher agreed energy; state specimen orientation if the project specifies it
Ultrasonic testing JB/T 4730.3, GB/T 2970 or GB/T 28297, with the acceptance class
Supplementary tests Simulated post-weld heat treatment, through-thickness or product analysis only when written on the order
Documentation Inspection document type required by the project, for example EN 10204 3.1 or 3.2
Other editions If GB/T 713.3-2023 or GB/T 713.4-2023 must also be met, say so on the enquiry; we review both editions before quoting

FAQ

Is 08Ni3DR in GB/T 713.3-2023?
No. In the 2023 revision 08Ni3DR moved to GB/T 713.4-2023, the nickel-steel part. GB/T 3531-2014 is the earlier edition that covered it together with the low-alloy grades.
What impact temperature does GB/T 3531-2014 08Ni3DR meet?
Table 2 requires 60 J minimum at -100°C for thicknesses from 6 mm to 100 mm.
What delivery conditions are allowed?
Normalized, normalized and tempered, or quenched and tempered, with tempering not lower than 600°C. Plate over 60 mm may be normalized, accelerated cooled and tempered by agreement.
Is 08Ni3DR the same as ASTM A203 Grade E?
No. Both are 3.5 % nickel steels, but strength, heat treatment and impact rules differ. Treat A203 Grade D or E as related grades and check the project specification.
What should a quotation enquiry include?
GB/T 3531-2014, grade 08Ni3DR, delivery condition, thickness by width by length, quantity, impact and ultrasonic requirements, any simulated PWHT, and the inspection document.

Request a quotation

Contact SHH STEEL for a quotation for GB/T 3531-2014 08Ni3DR low-temperature pressure vessel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

State the delivery condition, the Charpy test temperature and energy if they differ from Table 2, the ultrasonic testing standard and class, any simulated post-weld heat treatment, and the inspection document required by the project.

If you are considering ASTM A203 Grade D or E, or the GB/T 713.4-2023 version of 08Ni3DR, send the project specification. We will review the differences rather than assume the grades or editions are interchangeable.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X