JIS G3126 SLA325B Steel Plate | JIS G3126 Steel - SHH STEEL

JIS G3126 SLA325B Steel Plate

JIS G 3126 SLA325B is a carbon steel plate for low-temperature pressure vessels. Opened final JIS G 3126:2015 lists six types; SLA325B shares SLA325 chemistry and tensile values, but Table 7 sets colder impact temperatures. Applicable thickness is 6 mm to 38 mm. Table 1 lists −60 °C as a usual-service reference, not a crack-arrest rating. Figures follow that 2015 text. SHH STEEL produces and exports SLA325B plate to the ordered edition, delivery condition and dimensions.
Equivalent Grades:
Near names include ASME SA203 Grade D; not automatic substitutes.
Heat Treatment
Quenched and tempered; thermomechanical control by agreement.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is JIS G 3126 SLA325B plate?

We produce and export JIS G 3126 SLA325B as carbon steel plate for pressure vessels and pressure equipment used at low temperature.

The opened public final used for the figures on this page is JIS G 3126:2015. Bibliographic listings record JIS G 3126:2021 as a later revision dated 20 April 2021. A purchased 2021 booklet was not opened, and these figures are not a 2021 requirements guarantee. The opened 2015 text covers hot-rolled carbon steel plates for pressure vessels and pressure equipment used at low temperature, and it is based on ISO 9328-1:2011, ISO 9328-3:2011, ISO 9328-5:2011 and ISO 9328-6:2011 with modifications.

Opened Table 1 lists six types — SLA235A, SLA235B, SLA325A, SLA325B, SLA365 and SLA410. Applicable thickness is 6 mm to 38 mm for SLA325B. The A and B endings on SLA235 and SLA325 are toughness distinctions (lowest usual-service reference temperature and Table 7 impact-test temperature), not separate tensile classes. SLA365 and SLA410 have no A or B suffix. These symbols are carbon-steel types under JIS G 3126; they are not JIS G 3127 nickel low-temperature plates and not ASME SA203 nickel grades.

SLA325B shares opened Table 3 chemistry and Table 6 tensile values with SLA325A. The B suffix is the colder toughness class: Table 1 lists −60 °C as the usual-service reference temperature, and Table 7 sets colder impact-test temperatures than SLA325A. Numeric cells below come from the opened public final JIS G 3126:2015. They are not a guarantee of a later unopened booklet. Bibliographic listings record JIS G 3126:2021 as a later revision dated 20 April 2021. A purchased 2021 booklet was not opened. SLA325B is supplied as fine-grain killed steel.

SHH STEEL produces and exports JIS G 3126 SLA325B plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for JIS G 3126 SLA325B

Opened clause 3 and Table 1 identify SLA325B as one of six types of carbon steel plate for low-temperature pressure vessels. Applicable thickness is 6 mm to 38 mm. Table 1 lists −60 °C as the lowest usable temperature for usual service. Note a states that this reference does not apply when special performance is required to arrest brittle-crack propagation.

Opened clause 4.1 requires the plate to be manufactured from fine-grain killed steel. Opened Table 2 heat treatment for SLA325B is: Quenching and tempering. Thermomechanical control may be applied by agreement. Heat-treatment symbols added after the type are TMC for thermomechanical control, N for normalizing, Q for quenching and tempering, and SR for a test-piece treatment equivalent to post-weld heat treatment. Opened examples include SLA235BTMC, SLA325AN, SLA365Q and SLA235BN3SR.

SLA325B shares opened Table 3 chemistry and Table 6 tensile values with SLA325A. The B suffix is the colder toughness class: Table 1 lists −60 °C as the usual-service reference temperature, and Table 7 sets colder impact-test temperatures than SLA325A.

Ladle analysis to opened Table 3 is the chemical acceptance basis. A separate product-analysis table was not printed in the opened 2015 final. Unless otherwise specified at the time of order, the inspection document is JIS G 0415 symbol 3.1 (inspection certificate 3.1). Marking, unless items are omitted by agreement while the product remains identifiable, includes the type symbol and heat-treatment symbol, the heat or inspection number, dimensions to JIS G 3193 clause 3, and the manufacturer’s name or abbreviation.

Numeric cells below come from the opened public final JIS G 3126:2015. They are not a guarantee of a later unopened booklet. Bibliographic listings record JIS G 3126:2021 as a later revision dated 20 April 2021. A purchased 2021 booklet was not opened.

Chemical composition of JIS G 3126 SLA325B

Ladle (heat) analysis in Table 3 is the normative chemical acceptance basis on the opened 2015 final. Opened clause 10.1 takes analysis samples to JIS G 0404 and determines ladle analysis to JIS G 0320. Table 3 prints carbon, silicon, manganese, phosphorus and sulfur only. Nickel is not given a published window on that table. Note a allows other alloying elements to be added as necessary; clause 14 requires those added-element contents to be reported when note a is used. A separate product-analysis table was not printed.

Element Value (wt. %) Source opened for this cell
Carbon (C) 0.16 max Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 3 ladle analysis
Silicon (Si) 0.55 max Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 3 ladle analysis
Manganese (Mn) 0.80–1.60 Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 3 ladle analysis
Phosphorus (P) 0.015 max Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 3 ladle analysis
Sulfur (S) 0.010 max Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 3 ladle analysis

For SLA325B the opened ladle limits are as tabulated. Phosphorus is 0.015 % maximum and sulfur is 0.010 % maximum on every type in Table 3. These carbon and manganese windows are not the thickness-banded carbon maxima or the 0.70 % / 0.80 % manganese maxima published on the live ASME SA203 / ASTM A203 pages.

Opened clause 6 applies when SLA325A, SLA325B, SLA365 or SLA410 is supplied with thermomechanical control. Carbon equivalent for TMC SLA325B is 0.38 max (Table 4), calculated from ladle analysis as Ceq = C + Mn/6 + Si/24 + Ni/40 + Cr/5 + Mo/4 + V/14. By agreement, weld-cracking sensitivity composition may be used instead: PCM 0.23 max (Table 5), calculated as PCM = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B. When Ceq or PCM applies, clause 14 requires the alloy contents used in the formula to be reported.

Numeric cells below come from the opened public final JIS G 3126:2015. They are not a guarantee of a later unopened booklet. Bibliographic listings record JIS G 3126:2021 as a later revision dated 20 April 2021. A purchased 2021 booklet was not opened.

Tensile, bend and impact properties for JIS G 3126 SLA325B

Ambient tensile and bend properties below come from Table 6 of the opened 2015 final. The heading printed there is yield point or proof stress, tensile strength, elongation and bendability. After bending, the outside of the specimen shall not crack. Opened clause 10.2.1 allows the manufacturer to omit the bend test unless the purchaser specifies it, but the bendability requirement itself still applies.

Item Value Source opened for this cell
Yield point or proof stress, N/mm² min 325 Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 6
Tensile strength, N/mm² 440–560 Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 6
Elongation, % min, 6 mm to 16 mm inclusive (No. 5 specimen) 22 Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 6
Elongation, % min, over 16 mm (No. 5 specimen) 30 Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 6
Elongation, % min, over 20 mm (No. 4 specimen) 22 Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 6
Bend angle / inside radius / specimen 180° / 1.5 × thickness / No. 1, transverse to the rolling direction Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 6

Opened Table 7 sets Charpy V-notch test temperatures by thickness and specimen size for SLA325B. The absorbed-energy lower limit is one-half of the maximum absorbed energy, not a fixed joule value. Note b defines the maximum absorbed energy as the average of three specimens tested at a temperature where all three show 0 % brittle-fracture appearance. That determination is usually made at room temperature; if 0 % fracture appearance is not obtained, the temperature is raised and the test is repeated. A separate set of three specimens from the same heat, thickness and heat-treatment condition is taken to determine that maximum absorbed energy (clause 10.2.1 b) 2)). The Table 7 test itself uses three specimens, reported as their average, taken parallel to the final rolling direction unless otherwise specified.

Thickness Specimen (height × width) Impact-test temperature Source opened for this cell
6 mm to under 8.5 mm 10 × 5 mm −60 °C Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 7
8.5 mm to 12 mm inclusive 10 × 7.5 mm −50 °C Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 7
Over 12 mm to 20 mm inclusive 10 × 10 mm −45 °C Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 7
Over 20 mm 10 × 10 mm −55 °C Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 7
Absorbed-energy acceptance V-notch, rolling direction unless transverse testing is agreed One-half of the maximum absorbed energy (not a fixed joule number) Opened public final JIS G 3126:2015, kikakurui whole-page source (https://kikakurui.com/g3/G3126-2015-01.html), opened 8 November 2026 (Asia/Shanghai); Table 7 note b

Table 7 note a allows a lower agreed test temperature to replace the tabulated temperature. Note c allows transverse testing by agreement; if the purchaser then approves, the longitudinal test may be omitted. When an individual energy result is expected to exceed 80 % of the testing-machine capacity, opened clause 7.2 allows the manufacturer to use a JIS Z 2242 V-notch subsize specimen: 10 °C lower than the Table 7 temperature when changing from 10 × 10 mm to 10 × 7.5 mm, 20 °C lower when changing from 10 × 10 mm to 10 × 5 mm, and 10 °C lower when changing from 10 × 7.5 mm to 10 × 5 mm.

If an impact test fails but the three-specimen average is at least 85 % of the specified value, opened clause 12 b allows three further specimens from the same sample; the lot passes if the six-specimen average meets Table 7. Tensile or bend failures may be retested under JIS G 0404 9.8. Re-heat treatment followed by a new test is also permitted.

Numeric cells below come from the opened public final JIS G 3126:2015. They are not a guarantee of a later unopened booklet. Bibliographic listings record JIS G 3126:2021 as a later revision dated 20 April 2021. A purchased 2021 booklet was not opened.

Delivery conditions for JIS G 3126 SLA325B

Opened Table 2 states the heat treatment for SLA325B: Quenching and tempering. Thermomechanical control may be applied by agreement. The purchaser states on the order the heat treatment the manufacturer is to perform and, where needed, the test-piece heat-treatment conditions and the number of cycles (clause 4.2.1.2). Test-piece heat treatment is applied to a sample taken from the plate, and specimens are taken after that treatment (clause 4.2.1.3).

Heat-treatment symbols written after the type are TMC for thermomechanical control on the plate, N for normalizing, Q for quenching and tempering, and SR for a test-piece treatment equivalent to post-weld heat treatment. Opened examples include SLA235BTMC, SLA325AN, SLA365Q and SLA235BN3SR.

The purchase order should name SLA325B, the edition required, heat-treatment symbols, thickness within 6 mm to 38 mm, width and length, whether a recorded bend test is required, any extra test, and the inspection document required.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

The opened 2015 text does not itself set a welding procedure for SLA325B. Welding and thermal cutting should be qualified for the carbon-manganese analysis, thickness and the specified delivery condition (quenching and tempering, with thermomechanical control permitted only by agreement). When SLA325B is supplied with thermomechanical control, opened clause 6 and Tables 4 and 5 set carbon equivalent at 0.38 max or, by agreement, PCM at 0.23 max.

Do not assume an ASME SA203 or ASTM A203 welding procedure without a project review. Those live pages specify nickel windows (about 2.25 % or 3.5 % Ni) that opened Table 3 does not print for this carbon-steel type.

Repair welding requires the purchaser’s prior approval. This page does not publish a maximum service temperature.

Form, appearance, dimensions and thickness tolerances

Shape, dimensions, mass and their tolerances follow JIS G 3193 on the opened 2015 text, except that thickness tolerances follow Table 8. Length tolerances and cut-edge width tolerances default to JIS G 3193 tolerance A unless otherwise specified.

Appearance follows JIS G 3193 clause 7. Repair welding requires the purchaser’s prior approval. This page does not list stock sizes or mill capacity.

Applications and specification limits

We produce and export SLA325B as fine-grain killed carbon steel plate for pressure vessels and pressure equipment used at low temperature. That application wording follows the opened 2015 scope clause. Table 1 lists a lowest usual-service temperature of −60 °C for SLA325B; note a says that reference does not apply when special performance is required to arrest brittle-crack propagation. This page does not invent a maximum service temperature or a vessel-code acceptance package beyond what the order names.

JIS G 3126 is not a JIS G 3127 nickel low-temperature plate order, not a JIS G 3119 or JIS G 3120 order, and not an ASME SA203 or ASTM A203 order unless that later book is written on the enquiry.

Compare JIS G 3126 SLA325B with other steel plates

JIS G 3126 SLA325B is a carbon steel plate for pressure vessels for low temperature service. The comparison below is for selection only; these materials are not equivalents. ASME SA203 and ASTM A203 are near names used in low-temperature vessel work, but they are nickel steels with specified nickel windows, different carbon and manganese schedules, and typically normalized delivery for Grades A, B, D and E. Opened JIS G 3126 Table 3 does not specify nickel, and SLA325B is delivered by quenching and tempering, with thermomechanical control permitted only by agreement.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
JIS G 3126 SLA325B (this plate) Carbon steel; opened Table 3 prints C, Si, Mn, P and S only and does not publish a nickel window. Ladle C and Mn for this type are 0.16 max and 0.80–1.60 Quenched and tempered; thermomechanical control by agreement. Opened 2015 Table 6: yield point or proof stress at least 325 N/mm²; tensile strength 440–560 N/mm² Low-temperature carbon-steel pressure vessels specified to SLA325B An ASME SA203 or ASTM A203 nickel grade is not an automatic substitute
ASME SA203 Grade A steel plate Specified 2.25 % nickel plate; live heat analysis Ni 2.10–2.50 %, C 0.17 max at ≤ 50 mm, Mn 0.70 max at ≤ 50 mm Live page: Grades A, B, D and E are normalized Live published yield 255 MPa and tensile strength 450–585 MPa; heat-analysis nickel 2.10–2.50 % Low-temperature nickel vessel plate on the live SA203 Grade A page Near name only; specified nickel and different C/Mn and heat treatment mean it is not identical to this carbon-steel type
ASTM A203 Grade A steel plate Specified 2.25 % nickel plate; live heat analysis Ni 2.10–2.50 %, C 0.17 max at ≤ 50 mm, Mn 0.70 max at ≤ 50 mm Live page: plates of Grades A, B, D and E are normally delivered normalized Live published yield 255 MPa and tensile strength 450–585 MPa; heat-analysis nickel 2.10–2.50 % Low-temperature nickel vessel plate on the live A203 Grade A page Near name only; specified nickel and different C/Mn and heat treatment mean it is not identical to this carbon-steel type
ASME SA203 Grade D steel plate Specified 3.5 % nickel plate; live heat analysis Ni 3.25–3.75 %, C follows the lower Grade A carbon schedule, Mn 0.70 max at ≤ 50 mm Live page: Grades A, B, D and E are normalized Live published yield 255 MPa and tensile strength 450–585 MPa; heat-analysis nickel 3.25–3.50 % Low-temperature nickel vessel plate on the live SA203 Grade D page Near name only; specified nickel and different C/Mn and heat treatment mean it is not identical to this carbon-steel type

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. Confirm chemistry, heat treatment, thickness, tensile properties, toughness and any extra tests.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
Japan JIS G 3126:2015 (opened final) SLA325B This plate. Applicable thickness 6 mm to 38 mm; Opened 2015 Table 6: yield point or proof stress at least 325 N/mm²; tensile strength 440–560 N/mm². Table 1 usual-service reference −60 °C. This product
United States ASME SA-203/SA-203M (live page) SA203 Grade D Live published yield 255 MPa and tensile strength 450–585 MPa; heat-analysis nickel 3.25–3.75 %. Live chemistry specifies nickel and uses different C and Mn limits from opened Table 3. Near name only; not identical
United States ASTM A203/A203M (live companion page) A203 Grade D Companion ASTM name on the matching live A203 page; same nickel-steel distinction from this carbon-steel type. Near name only; not identical
China / other — — No separately verified GB plate counterpart was established as an automatic equivalent for SLA325B on this page. Do not assume a local low-temperature vessel name is a substitute

Why choose SHH STEEL for JIS G 3126 SLA325B

  • We produce and export JIS G 3126 SLA325B carbon steel plate for low-temperature pressure vessels
  • We review the enquiry for edition, type, heat-treatment symbols, dimensions, impact testing and extra tests
  • We keep JIS G 3126 carbon-steel types distinct from JIS G 3127 nickel plates and from ASME SA203 / ASTM A203
  • We match documentation to what the purchase order requires

How to enquire for JIS G 3126 SLA325B plate

Item What to specify
Standard and designation JIS G 3126 SLA325B and the edition required
Heat treatment Quenched and tempered; thermomechanical control by agreement. Add the symbols from the standard (TMC, N, Q, SR) as required
Product form and dimensions Plate, with required thickness, width and length (applicable thickness 6 mm to 38 mm)
Chemistry Ladle analysis to Table 3 of the named edition (C, Si, Mn, P and S as printed; no product-analysis table was opened in the 2015 final). Report any note-a added elements
Mechanical tests Yield point or proof stress, tensile strength, elongation and bendability to Table 6; bend test if specified; Charpy test to Table 7, with absorbed energy accepted at one-half of the maximum absorbed energy
Other tests Ultrasonic examination to JIS G 0801 or other extra tests only when written on the order
Documentation State the inspection document type required by the project (the opened 2015 text defaults to an inspection certificate 3.1 unless otherwise specified)

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

FAQ

Which edition of JIS G 3126 are these figures from?
The figures on this page come from the opened public final JIS G 3126:2015. Bibliographic listings record JIS G 3126:2021 as a later revision dated 20 April 2021. A purchased 2021 booklet was not opened. Name the edition required on the order.
How many types does the opened 2015 final list, and what do the A and B suffixes mean?
Opened Table 1 lists six types: SLA235A, SLA235B, SLA325A, SLA325B, SLA365 and SLA410. That is the formal 2015 inventory, not a mill subset. On SLA235 and SLA325, A and B share chemistry and tensile values; they differ by Table 1 usual-service reference temperature and by Table 7 impact-test temperature. SLA325B shares opened Table 3 chemistry and Table 6 tensile values with SLA325A. The B suffix is the colder toughness class: Table 1 lists −60 °C as the usual-service reference temperature, and Table 7 sets colder impact-test temperatures than SLA325A.
What impact test applies to SLA325B?
Opened Table 7 temperatures for SLA325B are 6 mm to under 8.5 mm (10 × 5 mm): −60 °C; 8.5 mm to 12 mm inclusive (10 × 7.5 mm): −50 °C; Over 12 mm to 20 mm inclusive (10 × 10 mm): −45 °C; Over 20 mm (10 × 10 mm): −55 °C. Acceptance is one-half of the maximum absorbed energy, not a fixed joule number. Maximum absorbed energy is the average of three specimens at a temperature where all three show 0 % brittle-fracture appearance, usually found at room temperature. Direction is parallel to rolling unless a transverse test is agreed.
Can ASME SA203 Grade D replace SLA325B?
Only after a project review. ASME SA203 Grade D is a near name used for low-temperature vessels, but the live page specifies a nickel window and different carbon and manganese limits, and Grades A, B, D and E are typically normalized. SLA325B is a JIS G 3126 carbon steel type delivered by quenching and tempering, with thermomechanical control permitted only by agreement, with no nickel window printed in opened Table 3. It is not an automatic substitute.
What should a quotation enquiry include?
JIS G 3126 SLA325B, the edition required, heat-treatment symbols (TMC, N, Q or SR as used in the standard), thickness by width by length within 6 mm to 38 mm, quantity, whether a recorded bend test is required, any extra test, and the inspection document required.

Request a quotation

Contact SHH STEEL for a quotation for JIS G 3126 SLA325B plate. Please include your required quantity, thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the edition required. Figures on this page follow the opened public final JIS G 3126:2015 and are not a guarantee of JIS G 3126:2021 requirements. Include the heat-treatment symbols and any impact or extra-test instructions. If your project requires a recorded bend test, ultrasonic examination or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment, strength and toughness. An ASME SA203 or ASTM A203 nickel grade is not by itself a substitute instruction.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X