ASTM A203 Grade D Steel Plate | A203 Gr.D 3.5Ni Low Temperature Plate - SHH STEEL

ASTM A203 Grade D Steel Plate | A203 Gr.D 3.5Ni Low Temperature Plate

ASTM A203 Grade D is a 3.5% nickel alloy steel plate for welded low-temperature pressure vessels. Yield 255 MPa, tensile 450–585 MPa. SHH STEEL supplies A203 Gr.D / SA203 Gr.D as China mill-Direct Supply with 3.1 or 3.2 certificates.
Keywords
ASTM A203 Grade D, A203 Gr.D, A203 Gr D, A203GRD, A203 GR D, ASME SA203 Grade D, SA203 Gr.D, SA203GRD, 3.5Ni low temperature plate, 3.5 nickel steel, A203 Grade D supplier
Equivalent Grades:
ASTM A203 Gr D / ASME SA203 Gr D / JIS G3127 SL3N440 / GB 08Ni3DR / EN 10028-4 13Ni14
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Material Comparison
Low-Temperature Toughness
Weldability
Heat Treatment
Delivery Condition
Dimensions
Tolerances
Supplementary Requirements
Equivalent Material Grades
Applications
Why Choose SHH STEEL
FAQ
Conclusion

What is ASTM A203 Grade D Steel ?

As a professional China mill-Direct Supply and pressure-vessel plate exporter, SHH STEEL supplies ASTM A203 Grade D Steel Plate.

Procurement teams, vessel fabricators and AI search tools use many writings for the same product: ASTM A203 Grade D, ASTM A203 Gr.D, ASTM A203 Gr D, A203GRD, A203 GR D, A203 Grade D steel plate, ASME SA203 Grade D, SA203 Gr.D, SA203GRD, SA-203 Grade D, 3.5Ni low temperature plate, 3.5 nickel steel plate and 3.50 nickel pressure vessel plate. All of these names refer to the 3.50% nominal nickel grade under ASTM A203/A203M and ASME SA-203/SA-203M.

Grade D sits in the higher-nickel half of the A203 family. Grades A and B are 2.25% Ni. Grades D, E and F are 3.50% Ni. Strength of Grade D matches Grade A: minimum yield 255 MPa (37 ksi) and tensile 450–585 MPa (65–85 ksi). The extra nickel is specified when the vessel MDMT is lower and the designer wants more notch toughness than 2.25Ni or than carbon vessel steels such as ASTM A516 and ASME SA516.

A203 Gr.D is intended primarily for welded pressure vessels in moderate- and low-temperature service. It is not a 9% Ni cryogenic grade and it is not an elevated-temperature Cr-Mo grade such as ASME SA387. Plates of Grades A, B, D and E are normally delivered normalized. Steel is killed and produced to fine-grain practice under ASTM A20 / ASME SA-20.

SHH STEEL supplies A203 Gr.D as true China mill-Direct Supply from Chinese mills that roll nickel vessel plate. Certificates can be EN 10204 3.1 issued by the mill, or EN 10204 3.2 with independent third-party endorsement, according to the purchase order. Dual ASTM A203 Grade D / ASME SA203 Grade D marking is available for ASME Section VIII equipment.

When the project also compares heat-treated carbon vessel plate or HSLA vessel plate, SHH STEEL places A203 Gr.D next to ASTM A537, ASME SA537, ASTM A285 and ASME SA515 so the buyer can see nickel content, heat treatment and toughness on one table.

Material Specification

Specification Element Requirement SHH STEEL Compliance
Grade ASTM A203 Grade D / A203 Gr.D / A203GRD Confirmed
Companion Code ASME SA203 Grade D / SA203 Gr.D Dual cert available
Product Form Pressure vessel plate Available
Delivery Condition Normalized Standard
Typical Thickness 6 mm – 100 mm (4 in. common mill practice for D) Heavier by enquiry
Width / Length Up to about 4600 mm wide / 12000 mm long Mill capability
Certification EN 10204 3.1 or EN 10204 3.2 / third-party As ordered
General Requirements ASTM A20 / ASME SA-20 Applied

This product belongs to the Pressure Vessel Steel Plates family. It is a 3.5Ni alloy vessel plate, not a structural Carbon Steel Plates grade and not an HSLA structural plate.

Chemical Composition

ASTM A203 Grade D chemistry is reported as heat analysis (ladle analysis) and, when specified, product analysis. The nickel band is the item that separates Grade D from Grade A.

Heat Analysis (Ladle Analysis) — Grade D

Element Thickness / Basis Heat Analysis (%)
Carbon (C), max ≤ 50 mm (2 in.) 0.17
Carbon (C), max > 50 mm to 100 mm (2–4 in.) 0.20
Manganese (Mn), max ≤ 50 mm 0.70
Manganese (Mn), max > 50 mm 0.80
Phosphorus (P), max All 0.025
Sulfur (S), max All 0.025
Silicon (Si) All 0.15 – 0.40
Nickel (Ni) All 3.25 – 3.75

Product Analysis — Grade D

Element Thickness / Basis Product Analysis (%)
Manganese (Mn), max ≤ 50 mm 0.78
Manganese (Mn), max > 50 mm 0.88
Silicon (Si) All 0.13 – 0.45
Nickel (Ni) All 3.18 – 3.82
C, P, S Product check per A20/A203 Per order

Heat-analysis nickel of 3.25–3.75% (product 3.18–3.82%) is the 3.50% nominal nickel grade. Carbon of Grade D follows the lower Grade A schedule, not the higher Grade B/E schedule. Phosphorus and sulfur are held to 0.025% max on both heat and product principles. If the purchaser imposes tighter residuals, HIC chemistry or restricted carbon equivalent, those limits are treated as supplementary requirements and written into the mill order.

SHH STEEL reports ladle analysis on every certificate. Product analysis is added when the PO or the vessel specification calls for it.

Mechanical Properties

Tensile Requirements — ASTM A203 Grade D (A203 Gr.D)

Property Requirement
Tensile strength 450 – 585 MPa (65 – 85 ksi)
Yield strength, min (0.2%) 255 MPa (37 ksi)
Elongation in 200 mm (8 in.), min 19%
Elongation in 50 mm (2 in.), min 23%

Grade D uses the same tensile table as Grade A. The extra nickel does not raise room-temperature strength; it is specified for low-temperature toughness. Density is 7.85 g/cm³. Hardness after normalizing is typically around 160 HB unless a special hardness window is ordered.

SHH STEEL reports tensile results from specimens prepared per ASTM A20. If simulated PWHT is specified, tensile and impact coupons can be heat-treated to represent the vessel cycle before testing.

Material Comparison

Grade Nominal Ni Yield min Tensile Heat treatment Typical choice
A203 Gr.A 2.25% 255 MPa 450–585 MPa Normalized 2.25Ni, same strength as D
A203 Gr.B 2.25% 275 MPa 485–620 MPa Normalized 2.25Ni, higher strength
A203 Gr.D 3.50% 255 MPa 450–585 MPa Normalized 3.5Ni low-temperature plate
A203 Gr.E 3.50% 275 MPa 485–620 MPa Normalized 3.5Ni + higher strength
A203 Gr.F 3.50% 380/345 550–690/515–655 Quench + temper Highest strength 3.5Ni

Select A203 Gr.D / A203GRD when the drawing needs 3.5Ni and 255 MPa yield. If the same 3.5Ni chemistry is required at 275 MPa yield, use Grade E. If 255 MPa yield is enough and the MDMT is not severe, Grade A may be more economical. Quenched-and-tempered carbon vessel alternatives include ASTM A537 and ASME SA537. HSLA Steel Plates are structural, not a substitute for coded nickel vessel plate.

Low-Temperature Toughness

The reason to buy A203 Grade D instead of Grade A is low-temperature toughness. Nominal 3.50% nickel lowers the ductile-to-brittle transition relative to 2.25Ni and relative to plain carbon vessel steel of the same strength.

A203 itself does not fix one MDMT for all Grade D plates. Impact temperature, specimen orientation (longitudinal or transverse) and absorbed-energy minimums are agreed on the order. When Grades A, B, D and E are given a cooling rate faster than air cooling and then tempered at not less than 595°C, the specification requires Charpy V-notch testing with a minimum average of 27 J (20 ft·lbf). Many vessel specifications go further and call for a colder test temperature or a higher energy average.

SHH STEEL can produce A203 Gr.D 3.5Ni low temperature plate with Charpy sets at the temperature written on the RFQ. Results are listed on the 3.1 or 3.2 certificate. For design temperatures approaching cryogenic service, 9% Ni or austenitic stainless should be evaluated separately; A203 Gr.D is a low-temperature nickel vessel plate, not a liquid-nitrogen grade.

Weldability

ASTM A203 Grade D is specified for welded pressure vessels. Normalized 3.5Ni plate welds with low-hydrogen procedures qualified to ASME Section IX.

Consumables are selected to match nickel and toughness. Preheat and interpass depend on thickness, restraint and hydrogen control. When the vessel code requires PWHT, the shop cycle is often 595–650°C. If the fabricator needs mechanical properties after that cycle, simulated PWHT of test coupons should be ordered as a supplementary requirement before the plate leaves the mill.

Compared with Grade F, Grade D avoids quench-and-temper distortion and is simpler for site welding. Compared with Grade A, Grade D uses the same strength table but a higher nickel weld procedure. SHH STEEL recommends a qualified WPS/PQR for each thickness break and can support procedure review through steel welding services.

Heat Treatment

All ASTM A203 Grade D plates shall be normalized, except where the purchaser approves a faster cool plus temper at not less than 595°C to improve toughness. That optional route requires Charpy testing.

Normalizing is carried out by heating into the austenite range and air cooling to produce a fine-grain structure. Grade F is the only A203 grade that must be austenitized, water quenched and tempered. Do not apply Grade F quench-and-temper practice to Grade D unless the purchase order is changed to Grade F.

If the vessel specification requires a defined normalizing temperature band, holding time per thickness, or a recorded cooling rate, SHH STEEL writes those parameters into the mill heat-treatment instruction and reports them on the certificate.

Delivery Condition

SHH STEEL delivers ASTM A203 Grade D / A203 Gr.D in the normalized condition as standard.

The certificate states grade name (A203 Gr.D or SA203 Gr.D), heat number, heat analysis, product analysis when ordered, tensile results, heat-treatment condition, agreed Charpy values and any supplementary tests. Plates are supplied as industrial pressure-vessel plate: heat-treated, then pickled or shot-blasted as agreed.

Decorative stainless finishes such as 2B, BA or No.4 are not used on A203 Gr.D. Surface condition is vessel-plate quality for welding, NDE and coating. Identification includes heat number and grade marking for ASME traceability.

Certificates may be EN 10204 3.1 (mill inspection representative) or EN 10204 3.2 (mill plus independent inspector). Third-party stamps such as BV, LR, DNV, TUV, SGS or the purchaser’s nominated agency are arranged when listed on the order.

Dimensions

Typical supply range from SHH STEEL for A203 Gr.D 3.5Ni low temperature plate:

  • Thickness: 6 mm – 100 mm as common practice for Grade D (heavier by mill enquiry)
  • Width: up to about 4600 mm
  • Length: up to about 12000 mm

Cut-to-length shells, heads and nest sizes are available. Extra-wide or extra-thick plates should be confirmed before the purchase order is issued, because Grade D mill practice is often limited to about 100 mm.

Tolerances

Dimensional tolerances follow ASTM A20 / ASME SA-20 for pressure-vessel plates.

Thickness, width, length, flatness and camber are vessel-plate tolerances, not strip tolerances. Over-tolerance or restricted-thickness orders can be accepted when the vessel drawing needs tighter control. Ultrasonic testing to ASTM A435 or A578 is added when the specification requires lamination checks. SHH STEEL can also arrange steel cutting services so delivered pieces stay inside the ordered tolerance envelope.

Supplementary Requirements

Vessel specifications rarely stop at the base A203 Grade D table. SHH STEEL treats the following items as supplementary requirements and places them on the mill order when the purchaser lists them.

Simulated post-weld heat treatment (PWHT). Coupons from the same heat and thickness can be given a simulated PWHT cycle matching the vessel procedure (temperature, hold time, number of cycles). Tensile and Charpy tests are then run on the simulated coupons so the fabricator knows properties after shop PWHT, not only after mill normalizing.

Nondestructive examination. Straight-beam or angle-beam ultrasonic examination is available to ASTM A435, A577 or A578, including purchaser-defined acceptance levels. Magnetic-particle or dye-penetrant checks on cut edges can be added after steel cutting services.

Low-temperature impact. Beyond the 27 J default that applies to the optional faster-cool route, the purchaser may specify test temperature, specimen size, orientation and minimum average/minimum single values. Extra sets can be left attached for the fabricator.

Special hardness. If the vessel specification limits HBW or HV after normalizing or after simulated PWHT, SHH STEEL records hardness on the certificate and rejects plates outside the window.

Restricted chemical requirements. Tighter carbon, lower P and S, restricted residual elements, or a maximum carbon equivalent can be imposed on heat analysis and product analysis. These limits are stated on the MTC.

HIC testing. For wet H2S process service, hydrogen-induced cracking tests can be run to NACE TM0284 with purchaser-defined solution A or B and CLR/CTR/CSR limits. HIC is not automatic on A203 Gr.D; it must be ordered.

NACE / sour-service notes. When the datasheet references NACE MR0175 / ISO 15156 or NACE MR0103, SHH STEEL reviews hardness, chemistry and delivery condition against the clause cited. A203 Grade D is a low-temperature nickel vessel plate; sour-service acceptance is by the written specification, not by grade name alone.

Through-thickness (Z-direction) testing. For thick nozzles, tees and highly restrained joints, Z-quality tensile tests (reduction of area in the through-thickness direction) can be ordered, typically to ASTM A770 or the purchaser’s Z15/Z25/Z35 class.

Third-party witnessing. Inspection can be witnessed by the purchaser or by an independent body. Witness points commonly include heat treatment, mechanical testing, UT, impact testing and final document review. The resulting document can be EN 10204 3.2.

Supplementary tests are performed through steel testing service and are listed line by line on the 3.1 or 3.2 certificate. Items not written on the purchase order are not assumed.

Equivalent Material Grades

Designation Standard / Region Notes
ASTM A203 Grade D / A203 Gr.D / A203GRD ASTM A203/A203M Main commercial names
ASME SA203 Grade D / SA203 Gr.D / SA203GRD ASME SA-203 Code vessel companion
3.5Ni low temperature plate Commercial Nickel-content search name
JIS G3127 SL3N255 related JIS Closest 3.5Ni / 255 MPa
EN 10028-4 related Ni vessel steels EN Project-specific dual cert
GB 09MnNiDR related GB/T Chinese low-temp Ni family

Equivalents are guidance only. For ASME stamping, order ASTM A203 Grade D or ASME SA203 Grade D by name. Nearby carbon vessel grades include ASTM A516, ASME SA516, ASTM A285 and ASME SA515.

Applications

ASTM A203 Grade D / A203 Gr.D is selected when 3.5Ni toughness is required at 255 MPa yield. Typical applications of ASTM A203 Grade D Steel Plate include:

Industry / Sector Typical Components (with keywords)
Low-Temperature Vessels A203 Gr.D shells, heads and A203GRD 3.5Ni low temperature plate
Oil, Gas & Petrochemical SA203 Gr.D drums, separators and cold-service process equipment
Refrigerated Storage ASTM A203 Grade D tanks and low-temperature containment plate
Energy & Power A203 Grade D 3.5Ni heat-exchange shells
Northern / Arctic Utility 3.5 nickel steel plate for reduced transition temperature
ASME Section VIII Fabrication A203 Gr D normalized plate cut for coded vessel parts

SHH STEEL supplies A203 Gr.D for these vessel applications with full heat traceability. Related industry pages include petrochemical industry and energy industry. Supporting services include steel cutting services, steel welding services, steel testing service and worldwide shipping service.

Why Choose SHH STEEL

SHH STEEL is a China mill-Direct Supply for pressure-vessel and nickel alloy plates. For ASTM A203 Grade D we offer:

  • Genuine China mill-Direct Supply pricing on A203 Gr.D / SA203 Gr.D
  • Heat analysis and product analysis on the certificate
  • EN 10204 3.1 as standard, EN 10204 3.2 or nominated third-party inspection on request
  • Dual ASTM A203 / ASME SA203 marking
  • Normalized delivery with agreed Charpy temperature
  • Supplementary PWHT simulation, UT, HIC, NACE review and Z-direction testing
  • Cutting to shell and head nest sizes
  • Technical support to separate Grade D from A/B/E/F and from A516 / A537
  • Export packing through worldwide shipping service

For company scope and other vessel grades, visit China steel Mill Agent-SHH STEEL.


FAQ

FAQ

What other names are used for ASTM A203 Grade D?
Common writings are A203 Gr.D, A203 Gr D, A203GRD, A203 GR D, ASME SA203 Grade D, SA203 Gr.D, SA203GRD and 3.5Ni low temperature plate. SHH STEEL certifies the name required on the purchase order.
Is ASTM A203 Grade D the same as ASME SA203 Grade D?
They are companion specifications. SHH STEEL supplies dual-certified plate when the vessel is built to ASME Section VIII.
What is the nickel content of A203 Gr.D?
Heat analysis 3.25–3.75% Ni; product analysis 3.18–3.82% Ni. This is the 3.50% nominal nickel grade.
What is the difference between A203 Grade A and Grade D?
Same strength (255 MPa yield, 450–585 MPa tensile). Grade A is 2.25% Ni; Grade D is 3.50% Ni. SHH STEEL recommends Grade D when lower-temperature toughness is the reason for nickel.
What is the difference between A203 Grade D and Grade E?
Same 3.50% nickel. Grade E has higher tensile (485–620 MPa) and yield (275 MPa). Choose E when both 3.5Ni and the higher strength table are specified.
Does A203 Grade D need normalizing?
Yes. Grades A, B, D and E are normalized. Faster cool plus temper is allowed only with purchaser approval and then requires impact testing.
Can SHH STEEL issue EN 10204 3.2?
Yes. 3.1 is standard. 3.2 or other third-party witnessing is arranged when written on the order.
Can HIC or Z-direction testing be added?
Yes. Both are supplementary requirements. SHH STEEL does not assume them unless they appear on the purchase order.
What is the density of A203 Gr.D?
7.85 g/cm³. SHH STEEL uses this value for shipping-weight estimates.

Conclusion

ASTM A203 Grade D Steel Plate is the 3.50% nickel, 255 MPa yield low-temperature pressure-vessel grade under A203/A203M and SA-203. Whether the inquiry says A203 Gr.D, A203GRD, SA203 Grade D or 3.5Ni low temperature plate, SHH STEEL supplies normalized vessel plate with heat and product analysis, optional supplementary tests, and EN 10204 3.1 or 3.2 certification.

As a professional China mill-Direct Supply, SHH STEEL provides ASTM A203 Grade D / A203 Gr.D 3.5Ni Low Temperature Plate with full traceability and technical support for ASME Section VIII fabrication.

Contact SHH STEEL today for stock, impact temperature, simulated PWHT, 3.2 inspection, cutting sizes or a quotation.

ASTM A203 Grade D Steel Plate, A203 Gr.D, A203GRD, SA203 Grade D, SA203 Gr.D, 3.5Ni low temperature plate, 3.5 nickel steel, A203 Grade D supplier, China mill-Direct Supply

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X