ASTM A312 UNS S30415 Stainless Steel Pipe | ASTM A312 Stainless Steel - SHH STEEL

ASTM A312 UNS S30415 Stainless Steel Pipe

ASTM A312 UNS S30415 heat-resisting austenitic stainless steel pipe in SML, WLD and HCW, with C 0.04–0.06%, Si 1.00–2.00%, N 0.12–0.18%, Ce 0.03–0.08%, an 87/42 ksi Table 4 floor and a 1900 °F anneal, supplied by SHH STEEL with EN 10204 3.1 MTCs.
Grade
UNS S30415
Standard
ASTM A312 / A312M
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASTM A312 UNS S30415 Stainless Steel Pipe

A312/A312M is the ASTM product specification for seamless, welded, and heavily cold-worked austenitic stainless steel pipe intended for high-temperature and general corrosive service. It stands on its own as an ASTM standard, and this page is written against it. UNS S30415 is one of the less common rows in its Table 1, and that is exactly why buyers ask us to spell out what the specification actually fixes for this alloy and what is left to agreement between purchaser and mill.

UNS S30415 is a heat-resisting austenitic alloy listed in A312 by UNS number only. It looks like a tightly controlled 304H at first glance, with 0.04–0.06% carbon, 18.0–19.0% chromium, and 9.0–10.0% nickel, but it adds 1.00–2.00% silicon, 0.12–0.18% nitrogen, and 0.03–0.08% cerium. Silicon and cerium improve oxidation resistance and scale adhesion, and nitrogen lifts the Table 4 floor to 87 ksi tensile and 42 ksi yield, so it is ordered for hot-gas and furnace service where 304H runs out of margin.

SHH STEEL can supply ASTM A312 UNS S30415 pipe as seamless (SML), welded (WLD), or heavily cold-worked (HCW) product, in ASME B36.19 stainless schedules or special OD and wall by agreement, with EN 10204 3.1 mill test certificates that report the full Table 1 heat analysis, the Table 4 tension results, and the heat-treatment record. Where a purchase order also asks for ASME SA-312 marking, dual marking can be offered on heats that qualify under both documents, but the ASTM grade remains the one this page describes.

The order should read ASTM A312 UNS S30415, because there is no TP name. The alloy is often known by a producer trade name, and European drawings may cite EN 1.4818, but both are cross-references; the contract chemistry is the Table 1 row, including the cerium band that a generic 304H certificate template will not have a line for.

If UNS S30415 turns out not to be the right fit, the closest sister pages in the same ASTM series are A312 UNS S30815, A312 TP304H, A312 UNS S30615, A312 TP309H, and A312 TP310H. All A312 grades are collected on the A312/A312M hub, so a short list can be compared against one standard before the enquiry goes out.

Manufacturing Types (SML / WLD / HCW)

ASTM A312 allows three manufacturing routes for UNS S30415 pipe, and the route is a purchase-order decision rather than a property of the grade. Whichever route is chosen, the heat must still meet the same Table 1 limits (C 0.04–0.06%, Mn ≤0.80%, Si 1.00–2.00%, Cr 18.0–19.0%, Ni 9.0–10.0%, N 0.12–0.18%, and Ce 0.03–0.08%), the same Table 4 tension floor, and the same 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling heat-treatment requirement before any length is released.

  • Seamless (SML) pierced and hot or cold finished, chosen for heavy wall, high pressure, or owner specifications that exclude a weld seam
  • Welded (WLD) formed from flat-rolled product and welded without filler or with filler where the edition allows, economical in thinner walls and larger diameters
  • Heavily cold-worked (HCW) welded pipe given at least 35% cold reduction of the weld and base metal before the final anneal, which refines the weld structure toward seamless behaviour

S30415 is a specialty heat-resisting alloy usually supplied seamless in small and medium sizes, while welded pipe is quoted against defined quantities and should come with a clear statement on filler use in the seam. Tell us which route your design code or client specification accepts, because a quotation that leaves the route open forces the mill to choose and can create disputes at receiving inspection.

Chemical Composition of ASTM A312 UNS S30415

The melting analysis in Table 1 is what the heat must meet when it is cast, and it is the first table a reviewer should compare against the mill certificate. For UNS S30415 the defining limits are C 0.04–0.06%, Mn ≤0.80%, Si 1.00–2.00%, Cr 18.0–19.0%, Ni 9.0–10.0%, N 0.12–0.18%, and Ce 0.03–0.08%. The table below reproduces the Table 1 row as published, with elements carrying no requirement shown as such rather than filled with invented values.

Element UNS S30415 melting analysis
Carbon (C) 0.04 – 0.06
Manganese (Mn) ≤ 0.80
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.030
Silicon (Si) 1.00 – 2.00
Chromium (Cr) 18.0 – 19.0
Nickel (Ni) 9.0 – 10.0
Nitrogen (N) 0.12 – 0.18
Cerium (Ce) 0.03 – 0.08
Molybdenum (Mo) … (no requirement)

Silicon, nitrogen, and cerium are the three lines that make this alloy what it is, and all three must be on the certificate. Manganese is held to 0.80% maximum, well below the 2.00% common for A312 grades, and the carbon window of 0.04–0.06% is narrower than TP304H, which gives more predictable creep behaviour.

Product analysis is a separate check made on the finished pipe, and ASTM A312 refers it to the permitted variations in ASTM A480 Table A1.1. The second table adds those tolerances to the melt limits so you can see the band that a check analysis on the pipe is allowed to fall within when Supplementary Requirement S1 or an owner check is ordered.

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) 0.04 – 0.06 0.01 under / over 0.03 – 0.07
Manganese (Mn) ≤ 0.80 0.03 over ≤ 0.83
Phosphorus (P) ≤ 0.045 0.010 over ≤ 0.055
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) 1.00 – 2.00 0.05 under / 0.10 over 0.95 – 2.10
Chromium (Cr) 18.0 – 19.0 0.20 under / over 17.80 – 19.20
Nickel (Ni) 9.0 – 10.0 0.10 under / over 8.90 – 10.10
Nitrogen (N) 0.12 – 0.18 0.01 under / over 0.11 – 0.19
Cerium (Ce) 0.03 – 0.08 Not listed in A480 Table A1.1 Not established—by agreement

Read the product limits as acceptance bounds for a check analysis only. A heat that sits outside the Table 1 melt range is non-conforming even if a later product analysis lands inside the widened band, so the certificate should always show the ladle analysis first. Cerium has no row in A480 Table A1.1, so a product tolerance for it is not established and any check analysis limit is by agreement.

Because S30415 is often compared with TP304H, the next table sets the two Table 1 rows side by side so the differences in silicon, nitrogen, and cerium are easy to see.

Element TP304H (S30409) S30415
C 0.04 – 0.10 0.04 – 0.06
Mn ≤ 2.00 ≤ 0.80
Si ≤ 1.00 1.00 – 2.00
Cr 18.0 – 20.0 18.0 – 19.0
Ni 8.0 – 11.0 9.0 – 10.0
N … 0.12 – 0.18
Ce … 0.03 – 0.08

Mechanical Properties of ASTM A312 UNS S30415

Table 4 sets the room-temperature tension requirements for UNS S30415: 87 ksi [600 MPa] tensile strength and 42 ksi [290 MPa] yield strength minimum, with elongation of 35% longitudinal / 25% transverse minimum. The table below shows those values in the form used on the specification, and the mill certificate should report actual results against each line.

Property (Table 4) UNS S30415
Tensile strength, min 87 ksi [600 MPa]
Yield strength (0.2% offset), min 42 ksi [290 MPa]
Elongation in 2 in. or 50 mm (or 4D), min 35% longitudinal / 25% transverse
Hardness No maximum in Table 4
Grain size Not listed in Table 5

The comparison below puts the S30415 Table 4 floor beside TP304, TP304H, and TP316 to show how much the nitrogen addition raises strength.

Grade UNS Tensile min, ksi [MPa] Yield min, ksi [MPa]
TP304 S30400 75 [515] 30 [205]
TP304H S30409 75 [515] 30 [205]
— S30415 87 [600] 42 [290]
TP316 S31600 75 [515] 30 [205]

The 42 ksi yield is 40% above the 30 ksi of TP304H, and at elevated temperature the alloy is designed to keep a strength advantage, which is why it is used for heater and furnace lines. Design allowables at temperature come from the governing code for S30415, not from Table 4, and Table 5 grain-size requirements do not apply to this UNS.

No hardness maximum is set for this grade in Table 4, so a hardness figure on a certificate is information rather than an acceptance criterion unless your order adds one. If a project specification imposes hardness or impact testing, write it on the purchase order so the mill can plan the test pieces before the pipe is cut.

Dimensions, Tolerances and Stock Sizes

Dimensions for ASTM A312 UNS S30415 pipe are normally ordered by NPS and schedule from ASME B36.19, or by outside diameter and wall where the design calls for a non-standard size. Outside-diameter tolerance and wall tolerance come from the specification itself, and wall is read as nominal unless Supplementary Requirement S8 asks for minimum wall. The permitted variations in wall thickness from Table 3 are shown below by NPS band and wall-to-diameter ratio.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

In practice the under-tolerance of 12.5% is the figure that matters for pressure design, because the designer has already sized the nominal wall with that allowance in mind. The over-tolerance varies with NPS and the wall-to-diameter ratio, which matters more for fit-up and weld preparation than for strength. For UNS S30415, whose higher strength or special chemistry often justifies a lighter or more closely engineered wall, confirm whether your calculation assumed nominal or minimum wall before the order is placed.

Stock / Available sizes. The table below shows the representative size band we quote for ASTM A312 UNS S30415, with example OD × wall combinations taken from B36.19 schedules. It is a supply and stock-enquiry range rather than a promise that every size sits on the floor today: for S30415 a limited range of seamless sizes in Sch 10S and 40S may be available from existing material, but most orders are planned as mill production. Special OD, special wall, and cut lengths are always handled on enquiry.

Representative size Example OD × wall Typical schedules / notes
NPS 1/2 – 2 21.34 × 2.77 mm (NPS 1/2 Sch 40S); 60.33 × 3.91 mm (NPS 2 Sch 40S) Sch 10S / 40S / 80S; small-bore process and instrument take-offs
NPS 2-1/2 – 6 88.90 × 5.49 mm (NPS 3 Sch 40S); 168.28 × 3.40 mm (NPS 6 Sch 10S) Sch 10S / 40S / 80S; the most frequent enquiry band
NPS 8 – 12 219.08 × 8.18 mm (NPS 8 Sch 40S); 323.85 × 4.57 mm (NPS 12 Sch 10S) Sch 10S / 40S; confirm SML or WLD route on enquiry
NPS 14 – 24 406.40 × 4.78 mm (NPS 16 Sch 10S); 609.60 × 9.53 mm (NPS 24 Sch 40S) Sch 10S / 40S; usually mill-order, mostly welded
Special OD × wall Any OD and wall the mill can qualify On enquiry: state OD, nominal or minimum wall, and length practice

Read the example sizes as orientation for writing the enquiry, not as a price list. When you send a size list we check live availability line by line, separate what can ship from existing material from what needs a mill slot, and give the lead time for each group so the purchase order can be split if the schedule demands it.

Equivalent Grades

Buyers often arrive with a trade name, a plate designation, or a European number rather than the A312 row. The table below maps the names we see on enquiries for UNS S30415, but only the ASTM A312 grade and UNS number are contractual on this page; everything else is a cross-reference that needs checking against its own standard.

Designation Notes
ASTM A312 UNS S30415 Governing grade on this page (no TP name)
ASME SA-312 UNS S30415 Separate Code standard; dual mark only when the order names both
EN 1.4818 Commonly cited European counterpart; verify against the EN standard
ASTM A240 / A213 S30415 Plate and tube counterparts under separate specifications
Producer trade names Order by UNS S30415, not by trade name

The ASME SA-312 row is listed because some Code projects require it, not because it is a synonym. ASME SA-312 is a separate standard adopted into the Boiler and Pressure Vessel Code, and the SA312 UNS S30415 page covers that document on its own terms. When both marks are wanted, the order should name both specifications and their editions so the certificate can state compliance with each.

Heat Treatment and Delivery Condition

S30415 is not individually listed in Table 2, so it takes the general row: solution anneal at 1900 °F [1040 °C] minimum, then quench in water or cool rapidly by other means, a capability shown by A262 Practice E when S7 is ordered. It is not one of the grades that must be reheated before quenching, so seamless pipe may be quenched directly after hot forming if it is not below the Table 2 minimum. Producers of this chemistry frequently anneal above 1900 °F to develop the intended grain structure, and the actual temperature should be recorded.

Delivery condition for UNS S30415 is solution annealed, then descaled by pickling or by blasting and pickling, straightened, and cut to the ordered length practice. HCW pipe receives its cold reduction before the final anneal, so cold work is never the delivered condition. Ask for the actual annealing temperature and cooling method to be recorded on the certificate, because a reviewer cannot otherwise confirm the Table 2 requirement from the document alone.

Corrosion Resistance

ASTM A312 contains no corrosion table, so the following is engineering commentary rather than a specification requirement. S30415 is designed for oxidation rather than aqueous corrosion. The silicon and cerium additions help form a dense, adherent oxide scale, and producer literature puts its useful oxidation limit around 1920 °F [1050 °C]; that figure is guidance, not an A312 requirement.

In aqueous service it behaves broadly like 304H, so it is not a choice for chloride-bearing water or strong acids. Long exposure in the sigma-forming temperature range can lead to some embrittlement as for other heat-resisting austenitics, and sulfur-bearing or carburizing atmospheres need a specific review rather than an assumption that the oxidation advantage carries over.

Applications of ASTM A312 UNS S30415 Pipe

Applications for ASTM A312 UNS S30415 pipe are mostly in elevated-temperature equipment where oxidation and strength both matter. The table below gives the typical uses, each subject to code confirmation for this UNS.

Application Role of S30415 Note
Furnace radiant and muffle tubes Oxidation resistance with high strength allows thinner walls Check code listing if pressure retaining
Recuperators and heat exchangers Thermal cycling resistance of the Ce-Si oxide Watch for condensate corrosion at cold end
Hot-gas ducting and stacks Lightweight welded pipe in hot flue gas Sulfur levels in fuel influence life
Petrochemical heaters Convection-section piping and supports Compare with TP304H or higher alloys
Kilns, calciners, incinerators Burner tubes, thermowells, protection tubes Abrasion and ash chemistry matter
Heat-treatment equipment Radiant tubes, retorts, fixtures made from pipe Carburizing atmospheres may need higher Ni

Treat the table as a starting point for discussion with the process licensor or corrosion engineer, not as an approval. Code allowable stresses, temperature limits, and any owner material lists decide whether UNS S30415 is acceptable on a given line, and those checks should be made before the pipe is ordered rather than after it arrives.

Weldability

S30415 is weldable by GTAW, GMAW, SMAW, and SAW with practices similar to other austenitic stainless steels, with attention to its silicon and nitrogen content and the hot-cracking tendency that higher silicon can bring. It is not listed in Table 6, so no AWS A5.9 class is assigned and filler choice is by agreement. Producers offer matching-chemistry consumables for full high-temperature performance; where a standard 308H or 309-type filler is used instead, the joint will reflect that filler’s oxidation and strength.

Qualify the procedure on UNS S30415 itself rather than on a convenient 304 coupon, because the qualification has to demonstrate the strength and soundness of this chemistry. Clean joint preparation, controlled heat input and interpass temperature, and a back-purged root are the normal baseline; the certificate for any WLD pipe should also state whether filler metal was used in the longitudinal seam.

Surface Finishes

Surface condition for ASTM A312 UNS S30415 pipe should be stated on the purchase order rather than left to mill default. On stainless pipe, residual scale, embedded free iron, and chloride contamination from handling can matter as much as the nominal finish name, and they are far easier to prevent at the mill than to correct on site.

  • Annealed and pickled the standard delivery after solution treatment for process piping
  • Blasted and pickled when heavier scale needs mechanical help before chemical descaling
  • Bright annealed by agreement, generally on smaller sizes where the furnace atmosphere can be controlled
  • Passivated or polished by agreement, with the method and acceptance criteria written on the order

For UNS S30415, a pickled surface is normal; bright finishes rarely matter in furnace service, but heavy scale left from hot finishing should be removed so the protective oxide can form evenly in service. If the line will be inspected for surface iron, specify the test method at the enquiry stage so that the packing and handling plan supports it.

Inspection and Testing

The base acceptance package for ASTM A312 UNS S30415 pipe combines heat analysis, tension testing, the flattening or bend test that applies to the manufacturing type, and a hydrostatic or non-destructive electric test on every length. Visual and dimensional inspection confirm the size and surface before marking. For S30415 the certificate must report silicon, nitrogen, and cerium along with carbon and the 42 ksi yield, because a standard 304H template omits cerium and that omission is a common cause of rejection.

Supplementary requirements are optional until they are written on the order. The options buyers request most often for this grade are summarized below, and each one adds test time that should be allowed for in the delivery schedule.

Option Use
S1 product analysis Confirms Si and N; Ce tolerance by agreement (not in A480)
S5 radiography Weld soundness on WLD pipe
Grain size report (PO) Optional for creep-sensitive applications
Elevated-temperature tensile (PO) Project-specific verification
PMI (OES preferred) Handheld XRF can confirm Cr/Ni/Si but not C, N, or reliably Ce

Third-party inspection, witness points, and EN 10204 3.2 certification are available when the order names the inspection agency. Agree the hold points before production starts, because witnessing a hydrotest or a tension test after the fact is not possible.

Packaging and Shipping

ASTM A312 UNS S30415 pipe is packed for handling and for ocean or land transport. Each length is marked with ASTM A312, the grade UNS S30415, the manufacturing type, size, heat number, and the test method used, with SA-312 added only when the order asks for dual marking. Bundle lists repeat the heat numbers so receiving can match pipe to certificates without opening every wrap.

  • End caps or bevel protectors fitted as ordered
  • Bundles strapped with protected contact points to limit iron pick-up
  • Wooden cases or seaworthy bundles for export, with moisture protection for sea freight
  • Small-bore or polished pipe cased separately where damage risk is higher

Stainless pipe should not be stored or lifted in contact with carbon steel, and for a specialty grade such as UNS S30415 it is worth keeping the material segregated by heat on arrival, since mixing it with common 304 stock is the most frequent cause of misuse on site.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless pipe, and for a specialty grade such as ASTM A312 UNS S30415 we quote against the edition you name rather than a generic catalogue sheet. We report the full Table 1 heat analysis, the Table 4 tension results, and the heat-treatment record, and we tell you early when a size or route is a mill order instead of letting the lead time surprise you.

  • Experience with UNS-only heat-resisting rows and the cerium and silicon lines they add to the certificate
  • Clear advice on sister grades under ASTM A312, so UNS S30415 is not confused with a commoner alloy that looks similar on paper
  • Honest separation of specification requirements from producer or market guidance in every document we send
  • EN 10204 3.1 certificates as standard, with third-party inspection and 3.2 certification on request

The aim is a delivery that clears receiving inspection on the first review. That means the certificate, the stencil, and the purchase order all say the same thing about grade, UNS number, manufacturing type, size, and heat treatment, and that any agreed variation is written down before the pipe is made.

Supply Capability

SHH STEEL can supply ASTM A312 UNS S30415 stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade, and each line can be narrowed to your project specification.

Item SHH STEEL capability for UNS S30415
Standard ASTM A312 / A312M, UNS S30415
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD and wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length Single random, double random, or cut to length
Heat treatment 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling
Filler guidance Not listed in Table 6; filler by agreement (matching or 308H/309-type, recorded on the WPS)
Testing Tension (87/42 ksi), flattening or bend, hydrostatic or electric test per length; S1, S5, S7, S8, S9 on order
Documents EN 10204 3.1 with full Table 1 analysis; 3.2 and third-party inspection on request
Trade terms FOB, CFR, CIF, EXW and other agreed Incoterms

Stock / Available sizes. The representative band for UNS S30415 is NPS 1/2 to 24 in Sch 10S, 40S, and 80S as listed under Dimensions. Selected common OD × wall combinations may be available from existing material, while heavy-wall seamless, unusual schedules, and special cut lengths are normally mill orders. We do not publish stock part numbers or tonnage claims for this grade; ask for a live check against your size list instead.

Enquiries move fastest when they state the A312 edition, UNS S30415, the manufacturing type, NPS or OD × wall (and whether the wall is nominal or minimum), length practice, finish, and any product-analysis, corrosion-test, or 3.2 requirements. Dual SA-312 marking, bevelled ends, and cut lengths are available on confirmed orders when the order says so.

FAQ

Is ASTM A312 UNS S30415 the same as ASME SA-312 UNS S30415?
They are two independent standards. ASTM A312/A312M is the ASTM product specification, and ASME SA-312 is the separate document adopted into the Boiler and Pressure Vessel Code. The technical rows for UNS S30415 are closely aligned in current editions, but a pipe is only certified to the document named on the order, so when both are needed the purchase order should list both specifications and editions and the certificate should state compliance with each.
What is the UNS number for ASTM A312 UNS S30415?
This alloy has no TP designation in A312 Table 1; it is ordered as UNS S30415 and is often described by a producer trade name in the market. The UNS number should appear on the mill certificate and on the stencil next to the ASTM A312 mark, because a trade name alone makes it hard for receiving inspection to tie the chemistry on the certificate to the pipe in the rack.
What are the tensile and yield requirements for ASTM A312 UNS S30415 pipe?
Table 4 requires 87 ksi [600 MPa] tensile strength and 42 ksi [290 MPa] yield strength minimum, with elongation of 35% longitudinal / 25% transverse minimum. These are room-temperature minimums for acceptance only; design allowables at temperature come from the applicable piping code, and they should be checked there before a wall thickness is fixed.
What heat treatment does ASTM A312 UNS S30415 pipe receive?
S30415 is not individually listed in Table 2, so it is solution annealed at the 1900 °F [1040 °C] minimum default and quenched or rapidly cooled; producers often anneal somewhat higher. The delivered condition is solution annealed and descaled, and the certificate should record the actual annealing temperature and the cooling method so a reviewer can confirm the requirement without asking the mill.
Which filler metal is used to weld ASTM A312 UNS S30415?
S30415 is not listed in Table 6, so ASTM A312 names no AWS A5.9 class; matching-chemistry consumables give the best high-temperature joint, and the choice must be agreed and recorded. Whatever is chosen should be recorded on the WPS and PQR, and the procedure should be qualified on UNS S30415 base metal so that the joint strength and soundness are demonstrated on the real chemistry.
Is ASTM A312 UNS S30415 pipe available seamless and welded?
Yes. ASTM A312 allows seamless (SML), welded (WLD), and heavily cold-worked (HCW) pipe for UNS S30415, all meeting the same chemistry, tension, and heat-treatment rules. Seamless is usual for heavy wall and high pressure, while welded is often more economical in thin walls and larger diameters; state the accepted route on the order.
What sizes of ASTM A312 UNS S30415 pipe can SHH STEEL supply?
We quote NPS 1/2 to 24 in Sch 10S, 40S, and 80S as the representative band, plus NPS 1/8 and up and special OD and wall by agreement. Some common sizes may be available from existing material, while heavy-wall seamless and unusual schedules are normally mill orders, so send a size list for a live check.
What documents come with ASTM A312 UNS S30415 pipe?
Each shipment carries an EN 10204 3.1 mill test certificate showing the A312 edition, UNS S30415, manufacturing type, heat number, the full Table 1 heat analysis, Table 4 tension results, heat treatment, and the hydrostatic or electric test. Third-party inspection and 3.2 certification can be added when the order names the agency.
How is UNS S30415 different from TP304H?
S30415 holds carbon to 0.04–0.06% and adds 1.00–2.00% silicon, 0.12–0.18% nitrogen, and 0.03–0.08% cerium, while keeping manganese to 0.80% maximum. The result is better oxidation resistance and an 87/42 ksi Table 4 floor against 75/30 ksi for TP304H.
What temperature can UNS S30415 pipe be used at?
ASTM A312 does not set a maximum service temperature. Producer literature cites oxidation resistance up to about 1920 °F [1050 °C], but the design limit comes from the governing code and the actual atmosphere, so treat that figure as guidance and confirm allowables for S30415.
Is S30415 a substitute for UNS S30815?
They are related but not interchangeable. S30815 has more chromium (20–22%) and nickel (10–12%) and a different Table 2 anneal, and it is aimed at higher temperatures. S30415 is a leaner step up from 304H; choose between them on temperature, atmosphere, and code listing.

Conclusion

ASTM A312 UNS S30415 (UNS S30415) is a UNS-only heat-resisting grade that improves on 304H with silicon, nitrogen, and cerium, giving an 87/42 ksi floor and better oxidation resistance for furnace and hot-gas service. The specification fixes C 0.04–0.06%, Mn ≤0.80%, Si 1.00–2.00%, Cr 18.0–19.0%, Ni 9.0–10.0%, N 0.12–0.18%, and Ce 0.03–0.08%, a Table 4 floor of 87 ksi [600 MPa] tensile and 42 ksi [290 MPa] yield, and 1900 °F [1040 °C] minimum solution anneal (Table 2 default) with rapid cooling heat treatment, while filler selection is by agreement because S30415 is not listed in Table 6. Put the manufacturing type, size and wall basis, finish, and any supplementary tests on the purchase order, and review the EN 10204 3.1 certificate against Tables 1, 2, and 4 before release. SHH STEEL can supply ASTM A312 UNS S30415 pipe to the edition you name; compare sister grades on the A312/A312M hub, or send your size list to admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X