ASME SA312 UNS S31655 Stainless Steel Pipe | SA 312/SA 312M
What is ASME SA312 UNS S31655 Stainless Steel Pipe
ASME SA-312/SA-312M covers seamless, welded and heavily cold-worked austenitic stainless steel pipe for high-temperature and general corrosive service, and it is technically aligned with ASTM A312/A312M of the referenced edition. UNS S31655 is listed in Table 1 without a TP designation. For pressure piping and code work, cite the grade, the UNS number and the edition of the standard on the purchase order and on the mill test certificate, rather than relying on a market label that several neighbouring grades share.
UNS S31655 is listed in Table 1 with no TP designation, so the UNS number is the grade name on every document. It is a high-chromium, nitrogen-alloyed austenitic grade with deliberately lean nickel: Cr 19.5–21.5%, Ni 8.0–9.5%, Mo 0.50–1.50%, N 0.14–0.25%, C ≤0.030%, S ≤0.015% and Cu ≤1.00%. The combination of high nitrogen and chromium supports a Table 4 row of 92 ksi [635 MPa] tensile and 45 ksi [310 MPa] yield, well above the 75/30 ksi of TP316 and the 80/35 ksi of TP316N. It is not an H grade. Table 2 does not list S31655 individually, so the default 1900 °F [1040 °C] anneal with rapid cooling applies, and Table 6 shows an ellipsis for the filler class, so the consumable is agreed on the WPS.
SHH STEEL can supply ASME SA312 UNS S31655 stainless steel pipe to the edition named on the enquiry, in seamless (SML), welded (WLD) and heavily cold-worked (HCW) forms. We cover ASME B36.19 schedules and special OD and wall combinations by agreement, issue EN 10204 3.1 mill test certificates as standard, and can dual-mark SA-312/A312 when the heat analysis, heat treatment, mechanical tests and marking satisfy both editions named on the purchase order. Tell us the NPS, wall or schedule, finish, length practice and any product-analysis or supplementary tests at enquiry stage, and we will confirm stock or mill rolling against those details.
Common commercial names and how they map to the ordered product are listed below. Use the full SA-312/A312 designation on the purchase order rather than market shorthand alone, because the shorthand is where grade substitutions usually start.
- UNS S31655 — unified numbering identity used on MTCs, stencils and ASME Section II Part D cross-references
- ASTM A312 S31655 / SA-312 S31655 — there is no TP name; the UNS must appear on the stencil and MTC
- “High-strength 316N” — a common mis-description; S31655 chemistry sits outside the TP316N envelope
S31655 is easy to mis-buy as a “high-strength 316N”. It is not a drop-in for ASME SA312 TP316N Stainless Steel Pipe, ASME SA312 TP316LN Stainless Steel Pipe, ASME SA312 TP317 Stainless Steel Pipe or ASME SA312 UNS S31726 Stainless Steel Pipe. Nickel at 8.0–9.5% and molybdenum at only 0.50–1.50% place it outside the TP316N envelope (Ni 10–14%, Mo 2–3%), even though the nitrogen looks familiar, and its 92/45 ksi row is its own. TP317 and S31726 are higher-molybdenum grades chosen for chloride resistance rather than strength. Hub: ASME SA 312/SA 312M.
Manufacturing Types (SML / WLD / HCW)
SA-312 defines three manufacturing routes that may be marked on finished UNS S31655 pipe. The route is a purchase-order decision driven by design code, size range, wall thickness and inspection preference. It does not change the Table 1 chemistry of UNS S31655, and every route must still finish with the solution anneal required by SA-312.
- Seamless (SML) — no welding at any stage. Preferred for small-bore and thick-wall pressure pipe, and wherever the piping class excludes welded product.
- Welded (WLD) — automatic welding without filler metal, finished so the pipe meets dimensional and mechanical requirements after final heat treatment. Common for larger NPS lines where the code accepts welded austenitic pipe.
- Heavily cold-worked (HCW) — welded pipe cold worked at least 35% in wall and weld before the final anneal, with the weld radiographed before cold work. Ordered when tighter OD and wall consistency matters.
Each finished length is hydrostatically tested or nondestructively electrically tested, and the manufacturer may choose the method unless the purchase order fixes one. Pipe NPS 10 and larger may ship marked “NH” only when the purchaser agrees to a system test instead. State SML, WLD or HCW explicitly on the enquiry; bids that differ only in manufacturing type are a common evaluation trap, and the same letters should appear on the stencil and the MTC.
Chemical Composition of SA312 UNS S31655
Melting analysis (heat / ladle analysis) — Table 1
The table below is the SA-312 Table 1 heat analysis for UNS S31655. Values are maximum unless a range is shown, and an ellipsis (…) means no requirement. These are the numbers the mill must report on the certificate, and they are the numbers receiving inspection should check first.
| Element | UNS S31655 melting analysis |
|---|---|
| Carbon (C) | ≤ 0.030 |
| Manganese (Mn) | ≤ 2.00 |
| Phosphorus (P) | ≤ 0.045 |
| Sulfur (S) | ≤ 0.015 |
| Silicon (Si) | ≤ 1.00 |
| Chromium (Cr) | 19.5 – 21.5 |
| Nickel (Ni) | 8.0 – 9.5 |
| Molybdenum (Mo) | 0.50 – 1.50 |
| Nitrogen (N) | 0.14 – 0.25 |
| Copper (Cu) | ≤ 1.00 |
Product analysis — A480/A480M Table A1.1 tolerances applied to Table 1
When product analysis is ordered (Supplementary Requirement S1 or PO wording), the check analysis may vary from the Table 1 limits by the A480 tolerances below. Product analysis is not automatic, so order it explicitly if your project needs it rather than assuming ladle values will satisfy the client inspector.
| Element | Melting (Table 1) | Tolerance (A480 A1.1) | Product analysis limit |
|---|---|---|---|
| Carbon (C) | ≤ 0.030 | 0.005 over | ≤ 0.035 |
| Manganese (Mn) | ≤ 2.00 | 0.04 over | ≤ 2.04 |
| Phosphorus (P) | ≤ 0.045 | 0.010 over | ≤ 0.055 |
| Sulfur (S) | ≤ 0.015 | 0.005 over | ≤ 0.020 |
| Silicon (Si) | ≤ 1.00 | 0.05 over | ≤ 1.05 |
| Chromium (Cr) | 19.5 – 21.5 | 0.20 under / 0.25 over | 19.30 – 21.75 |
| Nickel (Ni) | 8.0 – 9.5 | 0.10 under / over | 7.90 – 9.60 |
| Molybdenum (Mo) | 0.50 – 1.50 | 0.03 under / 0.05 over | 0.47 – 1.55 |
| Nitrogen (N) | 0.14 – 0.25 | 0.01 under / 0.02 over | 0.13 – 0.27 |
| Copper (Cu) | ≤ 1.00 | 0.05 over | ≤ 1.05 |
Read the S31655 certificate against its own row, not a 316 template. Chromium is higher than any 316 grade, nickel is lower, molybdenum is a modest 0.50–1.50% and nitrogen is a substantial 0.14–0.25%. Sulfur is tighter at 0.015% and copper carries a 1.00% maximum, so both must be reported. Product-analysis limits apply the A480 tolerances shown above. A heat certified with nickel above 9.5% or molybdenum above 1.50% is not S31655, however close it looks to a 316N analysis.
Mechanical Properties of SA312 UNS S31655
| Property | S31655 |
|---|---|
| Tensile, min | 92 ksi [635 MPa] |
| Yield, min | 45 ksi [310 MPa] |
| Elongation | 35% L / 25% T |
The 92/45 ksi row is a single line with no thickness split, and it is mandatory. Releasing S31655 against 80/35 or 75/30 criteria is a documentation error, and designers must take allowable stresses from the code tables for UNS S31655 rather than TP316 or TP316N rows. The higher yield can support thinner walls only after the governing code minimum thickness has been checked.
Actual certificate values are usually comfortably above the minima, but design and acceptance still use the Table 4 row unless the purchase order states higher guaranteed values. Record the row on the datasheet so fabricators and inspectors do not substitute a sister grade’s strength line from memory, and make sure the tension test on the MTC is traceable to the heat and lot that was shipped.
Dimensions and Tolerances
UNS S31655 pipe is normally ordered to ASME B36.19 schedules, with heavier B36.10 walls and special OD and wall combinations available by agreement. Wall thickness tolerance follows SA-312 Table 3, and outside diameter variations follow A999/A999M for the ordered size.
| NPS designator | Wall over | Wall under |
|---|---|---|
| 1/8 to 2-1/2 incl., all t/D | 20.0% | 12.5% |
| 3 to 18 incl., t/D up to 5% | 22.5% | 12.5% |
| 3 to 18 incl., t/D over 5% | 15.0% | 12.5% |
| 20 and larger, welded, all t/D | 17.5% | 12.5% |
| 20 and larger, seamless, t/D up to 5% | 22.5% | 12.5% |
| 20 and larger, seamless, t/D over 5% | 15.0% | 12.5% |
Source: SA-312 Table 3; outside diameter variations per A999/A999M. Cut lengths should not be shorter than ordered, and random or fixed length practice should be stated on the enquiry. Special walls and non-standard sizes need written mill agreement before rolling slots are booked, so raise them early if your design does not fit a standard schedule.
Equivalent Grades
| Designation | Notes |
|---|---|
| ASME SA-312 UNS S31655 | Governing specification for ASME code work |
| ASTM A312 UNS S31655 | Same chemistry and tensile rows for the referenced edition |
| UNS S31655 | Unified numbering identity on MTC and stencil |
Cross-references to EN or other national numbers are not given here, because SA-312 does not define them and near-equivalents rarely match every Table 1 limit. If a project needs a cross-standard equivalence, treat it as an engineering decision against both specifications rather than a catalogue lookup. Dual SA-312/A312 certification is straightforward when both editions are named on the order. Related grades for comparison: ASME SA312 TP316 Stainless Steel Pipe, ASME SA312 TP316L Stainless Steel Pipe, ASME SA312 TP316N Stainless Steel Pipe, ASME SA312 TP316LN Stainless Steel Pipe, ASME SA312 TP317 Stainless Steel Pipe, ASME SA312 UNS S31726 Stainless Steel Pipe.
Heat Treatment and Delivery Condition
UNS S31655 is not individually listed in Table 2, so the default solution-annealing practice applies: heat to a minimum of 1900 °F [1040 °C] and cool rapidly. UNS S31655 is not an H grade, so there is no Table 5 grain-size requirement and no clause 6.2 reheat rule. Pipe is delivered in the solution-annealed condition, and the certificate should state the heat-treatment temperature and cooling method actually used.
Fabricators who hot form or heavily cold work UNS S31655 bends and fittings should re-anneal to the same practice where the governing code requires it. Cite the ordered edition’s Table 2 default on the enquiry so the mill does not apply a neighbouring grade’s anneal by habit.
Corrosion Resistance
Higher chromium and nitrogen help pitting resistance compared with lean austenitic grades, but molybdenum tops out at 1.50%, so S31655 is not a 4–6% Mo chloride grade. For aggressive chlorides or warm seawater, grades such as ASME SA312 UNS S31726 Stainless Steel Pipe or ASME SA312 UNS S31254 Stainless Steel Pipe belong in the comparison. SA-312 publishes no corrosion rates, so service suitability for the actual medium, temperature and crevice geometry needs engineering review.
Intergranular-corrosion testing to A262 or similar is a supplementary requirement and applies only when written on the purchase order, so state the practice and acceptance criteria if your client needs it. The same applies to any pitting or crevice tests requested by the end user.
Applications of SA312 UNS S31655 Pipe
| Application | Why UNS S31655 | Buyer note |
|---|---|---|
| Pressure piping where a high yield floor saves wall | 92/45 ksi Table 4 row | Use code allowables for S31655 |
| General corrosive service needing more strength than 316N | High Cr and N, lean Ni | Not a high-Mo chloride grade |
| Projects naming S31655 on the datasheet | UNS-only identity | Stencil and MTC must show UNS S31655 |
S31655 tends to be specified by designers who want a strength step above TP316N without moving to duplex, and who can accept moderate molybdenum. Because there is no TP name, it is less widely stocked than the 316 family, and enquiries should state the UNS, the 92/45 ksi row and the sizes early so mill availability can be checked before need dates are fixed.
Weldability
Table 6 shows an ellipsis for the S31655 filler class, so there is no standard mapping to rely on. The consumable must be agreed and frozen on the WPS and PQR, and the procedure qualified on S31655 base metal, with attention to dilution of the lean nickel and high nitrogen. Mill longitudinal welds on WLD and HCW pipe are autogenous and use no filler.
Use stainless-only tooling and back-purge root passes where the specification calls for a clean root, and keep consumable lot records with the weld traveler when Section IX or B31 documentation applies. NDE extent for girth welds is a fabrication-code decision, separate from the mill hydro or electric test on each length.
Surface Finishes
Most UNS S31655 pipe ships pickled and passivated after the solution anneal, which is the normal finish for process piping. Other finishes are order extras and should be stated on the enquiry, together with whether a roughness target applies to the OD, the ID or both.
- Annealed and pickled (standard)
- Bright annealed, by agreement
- Mechanically polished OD, by agreement
- Electropolished ID for hygienic service, by agreement
Inspection and Testing
SA-312 sets the minimum test package for every heat and length of UNS S31655. Supplementary tests are only applied when written on the order, so the inspection and test plan should list them before production starts.
- Heat analysis to Table 1, including every element with a limit
- Tension test to the Table 4 row (92 ksi [635 MPa] / 45 ksi [310 MPa])
- Flattening and, for welded pipe, the applicable weld tests
- Hydrostatic or nondestructive electric test on each length
- Visual and dimensional checks to Table 3 and A999
- Optional: product analysis, IGC test, PMI, UT/RT of welds, EN 10204 3.2 witness
Packaging and Shipping
Each length is marked with SA-312 (and A312 when dual-certified), UNS S31655, the manufacturing type, size, heat number and test method. For export, we pack in a way that protects the stainless surface from carbon steel contact and moisture during ocean transit.
- Plastic end caps on every length
- Bundles strapped with non-metallic or protected bands
- Seaworthy wooden cases or crates for polished or thin-wall pipe
- Segregation from sister grades so stencils cannot be mixed
Why Choose SHH STEEL
SHH STEEL works with qualified stainless mills to supply UNS S31655 to the edition you name, and our job is to make sure what arrives on site matches the datasheet. That starts with reading the enquiry against the actual SA-312 rows—Table 1 chemistry, the 92 ksi [635 MPa] / 45 ksi [310 MPa] Table 4 row and the Table 2 anneal—and flagging mismatches before an order is placed. We are honest where the standard is silent: if Table 6 does not give a clear filler class, we say so rather than inventing one.
- Seamless, welded and HCW UNS S31655 to SA-312/A312, with dual marking when both editions are ordered
- EN 10204 3.1 MTCs as standard; 3.2 and third-party witness by arrangement
- Full Table 1 reporting, including nitrogen on every heat
- B36.19 schedules plus special OD and wall by agreement
- Export packing and heat traceability from mill to site
Supply Capability
We supply UNS S31655 pipe from mill production and selected stock, with lead time depending on size, wall and manufacturing type. The table summarises what we can offer; please confirm the details for your order on enquiry.
| Item | Supply |
|---|---|
| Grade | UNS S31655 |
| Standard | ASME SA-312/SA-312M, ASTM A312/A312M (dual by agreement) |
| Routes | SML, WLD, HCW |
| Sizes | ASME B36.19 schedules; special OD and wall by agreement |
| Filler guidance | by agreement (Table 6 shows “…”) |
| Certificates | EN 10204 3.1; 3.2 by arrangement |
Standard schedules can often ship from stock or short mill runs, while heavy-wall seamless and special sizes need a rolling slot. Send the edition, grade and UNS, size list, quantities and required date, and we will separate stock lengths from made-to-order items in our quotation so your site dates are realistic.
FAQ
-
Is ASME SA312 the same as ASTM A312?
- For chemistry, tensile requirements, manufacturing types and most testing language, ASME SA-312/SA-312M matches ASTM A312/A312M of the referenced edition. Dual SA312/A312 marking for UNS S31655 is common when ordered. Name both editions on the purchase order and the certificate so inspectors can verify the heat against the exact books you cited; a bare market stamp does not prove dual certification.
-
What is the UNS number for this grade?
- Table 1 lists UNS S31655 as UNS S31655, with no TP name. Use that UNS on the purchase order, the stencil and the MTC so the chemistry and tensile rows stay unambiguous. When a project mixes plate, fittings and pipe, carry the same UNS language across all forms, but still order pipe to SA-312/A312 rather than to a plate specification.
-
UNS S31655 vs TP316N — which should I order?
- TP316N keeps the 316 envelope (Ni 10–14%, Mo 2–3%) with N 0.10–0.16% and 80/35 ksi floors. S31655 has higher Cr 19.5–21.5%, leaner Ni 8.0–9.5%, Mo only 0.50–1.50%, N 0.14–0.25% and a 92/45 ksi row. Choose S31655 for strength when moderate Mo is acceptable, and TP316N when the corrosion basis is standard 316.
-
UNS S31655 vs TP316LN — which should I order?
- TP316LN is a low-carbon 316 with N 0.10–0.16%, Mo 2–3% and 75/30 ksi floors, aimed at welded aqueous service. S31655 also has low carbon (≤0.030%) but much higher strength at 92/45 ksi and less molybdenum. Pick TP316LN where the 316 corrosion basis governs and S31655 where wall weight and strength drive the design.
-
Seamless vs welded UNS S31655 — which is better?
- Neither is universally better. Seamless suits small-bore, thick-wall and pressure parts where the piping class excludes welds, while welded and HCW pipe are economical for larger sizes and offer good wall consistency. Choose the route your design code and datasheet allow, state SML, WLD or HCW on the order, and confirm the same letters on the marking and certificate.
-
Hydrostatic test vs NDE — which do I get?
- Each length of UNS S31655 is either hydrotested or nondestructively electrically tested, and the manufacturer may choose unless the purchase order fixes the method. If your piping class or client specification requires one method, state it on the order and check that the chosen test appears on the certificate for every length; a silent mill choice is not an approved project method.
-
What heat treatment applies to UNS S31655?
- UNS S31655 is not individually listed in Table 2, so the default solution anneal at a minimum of 1900 °F [1040 °C] with rapid cooling applies. UNS S31655 is not an H grade, so there is no Table 5 grain-size rule. Delivery is in the solution-annealed condition, and the certificate should state the temperature and cooling used so the record is complete.
-
What Table 1 chemistry defines UNS S31655?
- Table 1 for UNS S31655: C ≤0.030%, Mn ≤2.00%, P ≤0.045%, S ≤0.015%, Si ≤1.00%, Cr 19.5–21.5%, Ni 8.0–9.5%, Mo 0.50–1.50%, N 0.14–0.25% and Cu ≤1.00%. These are melting-analysis limits from the ordered edition, so do not invent tighter catalogue windows. When product analysis is needed, order it explicitly through Supplementary Requirement S1 or PO wording, and the A480 tolerances shown in the chemistry section then apply.
-
What are the Table 4 tensile requirements for UNS S31655?
- Table 4 minima for UNS S31655 are 92 ksi [635 MPa] tensile and 45 ksi [310 MPa] yield, with elongation of 35% longitudinal and 25% transverse. Actual certificate values are usually higher, but design and acceptance use Table 4 unless the order states higher guarantees. Record the row on the datasheet so nobody substitutes a sister grade’s line from memory.
-
What filler metal should I use to weld UNS S31655 pipe?
- Table 6 shows an ellipsis (“…”) for the filler class of S31655, so filler is by agreement. Freeze the AWS or EN class on the WPS and PQR before production welding and qualify the procedure on UNS S31655 base metal. Mill longitudinal welds on WLD and HCW pipe are autogenous, so Table 6 guidance applies only to joints made with filler, not to the mill seam.
-
Does UNS S31655 have a TP grade name?
- No. Table 1 lists UNS S31655 without a TP designation, so the UNS number is the grade identity on the purchase order, the stencil and the MTC. Market names such as “high-strength 316N” are misleading because the chemistry sits outside the TP316N row; insist on S31655 wording throughout so receiving inspection checks the correct Table 1 and Table 4 rows.
-
Why is sulfur limited to 0.015% in UNS S31655?
- Table 1 sets sulfur at 0.015% maximum for S31655, tighter than the 0.030% common on 316 grades. Tighter sulfur generally supports cleaner steel and weldability, and for buyers the practical rule is simple: the certificate must report sulfur at or below 0.015%, with product analysis allowed the A480 tolerance shown in the chemistry section.
Conclusion
ASME SA312 UNS S31655 is a high-Cr, nitrogen-alloyed, lean-nickel austenitic pipe grade with no TP name: C ≤0.030%, Cr 19.5–21.5%, Ni 8.0–9.5%, Mo 0.50–1.50%, N 0.14–0.25%, S ≤0.015% and Cu ≤1.00%, released against 92/45 ksi Table 4 minima with a Table 2 default 1900 °F [1040 °C] anneal. Table 6 gives no filler class, so the consumable is agreed on the WPS. It is not a high-strength TP316N. State the UNS, manufacturing type, schedule or wall and finish on the enquiry, and ask for the heat certificate with the full Table 1 analysis. For stock checks, mill certificates or dual SA-312/A312 supply questions, contact SHH STEEL at admin@steelspecs.com or browse the ASME SA 312/SA 312M category.