ASME SA312 TP316Ti / UNS S31635 titanium-stabilized stainless steel pipe in SML, WLD and HCW, with Mo 2.00–3.00%, Ti 5 × (C+N) minimum to 0.70% maximum and Si ≤0.75%, a 75/30 ksi Table 4 floor and a 1900 °F anneal, supplied by SHH STEEL with EN 10204 3.1 MTCs.
Grade
TP316Ti / UNS S31635
Standard
ASME SA312 / SA 312M (ASTM A312 / A312M)
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Dimensions
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA312 TP316Ti Stainless Steel Pipe

ASME SA-312/SA-312M covers seamless, welded, and heavily cold-worked austenitic stainless steel pipe for high-temperature and general corrosive service. TP316Ti / UNS S31635 is the titanium-stabilized member of the molybdenum-bearing 316 family. Table 1 sets C ≤0.08%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤0.75% (tighter than the 1.00% of most 316 grades), Cr 16.0–18.0%, Ni 10.0–14.0%, Mo 2.00–3.00%, N ≤0.10%, and Ti 5 × (C+N) minimum, 0.70% maximum. The titanium requirement is a formula rather than a fixed window, so whether a heat qualifies depends on its own carbon and nitrogen values.

Titanium combines with carbon and nitrogen to form stable titanium carbonitrides, so less carbon is left to form chromium carbides at grain boundaries after welding or exposure in the sensitizing range. That gives TP316Ti good resistance to intergranular corrosion while keeping the 2–3% molybdenum that helps in many chloride process duties. It is not an H grade: there is no 0.04% carbon minimum, no Table 5 grain-size rule, and no clause 6.2 reheat. Table 4 sets 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield with 35% longitudinal / 25% transverse elongation. TP316Ti is not individually listed in Table 2, so the 1900 °F [1040 °C] default solution anneal applies, and Table 6 in the extracted edition assigns no AWS filler class, so the consumable is by agreement. The grade is especially familiar to buyers working to European practice, where 1.4571 is a very common choice.

SHH STEEL can supply ASME SA312 TP316Ti stainless steel pipe to the edition named on the enquiry, in seamless (SML), welded (WLD), and heavily cold-worked (HCW) form. We quote ASME B36.19 schedules and special OD/wall by agreement, ship with EN 10204 3.1 mill test certificates that report C, N, and Ti as actual values so the 5 × (C+N) ratio can be checked, state the 75/30 ksi results and the 1900 °F anneal, and offer dual SA-312/A312 marking when chemistry, heat treatment, mechanical tests, and marking satisfy both editions on the purchase order. Please confirm NPS, wall or schedule, finish, length practice, filler basis, and any product-analysis or S7 test requirement when you enquire.

The names below are the ones buyers commonly use and how they map to the ordered product. Always put the TP name and UNS number on the purchase order.

  • ASME SA312 TP316Ti / UNS S31635 — preferred marking language for ASME-code and dual-marked pipe
  • ASTM A312 TP316Ti — same grade tables when the ASTM edition is referenced
  • EN 1.4571 / X6CrNiMoTi17-12-2 — the closest European grade; a useful map, but recheck the Ti formula, Si ≤0.75%, and the tensile floor before dual certifying
  • “316Ti” — common shorthand; acceptable in conversation, but the MTC must show C, N, and Ti

Sister grades buyers compare with TP316Ti include ASME SA312 TP316L Stainless Steel Pipe (C ≤0.035% with no titanium, 70/25 ksi), ASME SA312 TP316 Stainless Steel Pipe (no stabilization), ASME SA312 TP316H Stainless Steel Pipe (carbon band and H-grade rules for creep service), ASME SA312 TP321 Stainless Steel Pipe (titanium-stabilized with no molybdenum requirement), and ASME SA312 UNS S31272 Stainless Steel Pipe (fixed Ti 0.30–0.60% plus boron, lower Cr and Mo). Grade hub: ASME SA 312/SA 312M.

Manufacturing Types (SML / WLD / HCW)

ASME SA-312 recognizes three manufacturing routes for TP316Ti pipe, and the route is a purchase-order decision driven by the design code, the size range, wall thickness, and how the owner wants the pipe inspected. The route never changes the chemistry: whichever way the pipe is made, the heat must still meet C ≤0.08%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤0.75%, Cr 16.0–18.0%, Ni 10.0–14.0%, Mo 2.00–3.00%, N ≤0.10%, and Ti 5 × (C+N) minimum, 0.70% maximum, and every length must still go through the solution anneal at 1900 °F [1040 °C] minimum before it is released.

  • Seamless (SML) — no welding at any stage. Seamless is typical for higher-pressure process lines, heat-exchanger service, and heavy walls where the project excludes welded pipe. Every length must still receive the 1900 °F solution anneal with rapid cooling.
  • Welded (WLD) — automatic welding without filler metal, with the weld finished so the pipe meets dimensional and mechanical requirements after the final heat treatment. The strip or plate heat must itself carry the full TP316Ti chemistry, so ask for the coil or plate heat number on the certificate.
  • Heavily cold-worked (HCW) — welded pipe cold worked to at least 35% reduction of wall and weld before the final anneal, again without filler in the longitudinal seam, with the weld radiographed before cold work. Order HCW when the project specifically wants that marking and the process controls SA-312 writes around it.

Every finished length is hydrostatically tested or nondestructively electrically tested, and the mill may choose the method unless the purchase order fixes one. Pipe NPS 10 and larger may ship marked “NH” only when the purchaser accepts a system test in place of the hydrotest, and lots for mechanical testing follow clause 11.1. Clause 17 heat-treatment lot marking is not mandatory because TP316Ti is not an H grade, but many chemical-process owners still ask for heat and lot identity on the stencil. Titanium can form surface stringers and inclusions on poorly controlled heats, so for polished or critical-finish pipe it is worth asking the mill about its melting and inclusion practice.

TP316Ti is a mainstream grade in Europe but less commonly stocked in ASME markets than ASME SA312 TP316L Stainless Steel Pipe, so mill runs are typical for anything beyond common sizes. Enquire with route, sizes, wall, edition year, and whether you need EN 1.4571 dual marking, so the mill can plan a heat whose Ti, Si, and tensile results satisfy every standard named on the order.

Chemical Composition of SA312 TP316Ti

Two chemistry layers matter for TP316Ti. The melting (heat or ladle) analysis is mandatory for every heat under SA-312/A312 Table 1, while product analysis on finished pipe applies only when it is ordered through Supplementary Requirement S1 or purchase-order wording. Product tolerances are not printed in SA-312 itself; they come through ASTM A999/A999M §6.3 from ASTM A480/A480M Table A1.1. SHH STEEL reports the actual ladle values and, when ordered, the product values, and never quotes tighter catalogue windows that the standard does not publish.

Melting analysis (heat / ladle analysis) — Table 1

The table below is the heat analysis for TP316Ti from SA-312/SA-312M Table 1. Values are maximum unless a range is shown, and an ellipsis (…) means the ordered edition sets no requirement for that element. The titanium requirement is the Table 1 cell and footnote: Ti 5 × (C+N) min, 0.70 max.

Element TP316Ti / UNS S31635 melting analysis
Carbon (C) ≤ 0.08
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.030
Silicon (Si) ≤ 0.75
Chromium (Cr) 16.0 – 18.0
Nickel (Ni) 10.0 – 14.0
Molybdenum (Mo) 2.00 – 3.00
Titanium (Ti) 5 × (C+N) min, 0.70 max
Nitrogen (N) ≤ 0.10

Product analysis — A480/A480M Table A1.1 tolerances applied to Table 1

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) ≤ 0.08 0.01 over ≤ 0.09
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.045 0.010 over ≤ 0.055
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) ≤ 0.75 0.05 over ≤ 0.80
Chromium (Cr) 16.0 – 18.0 0.20 under / over 15.80 – 18.20
Nickel (Ni) 10.0 – 14.0 0.15 under / over 9.85 – 14.15
Molybdenum (Mo) 2.00 – 3.00 0.10 under / over 1.90 – 3.10
Titanium (Ti) 5 × (C+N) min, 0.70 max 0.05 over on max (Ti to 1.00 band) max ≤ 0.75 product; min tied to heat C+N
Nitrogen (N) ≤ 0.10 0.01 over ≤ 0.11

Source: SA-312 Table 1 TP316Ti / S31635. Ti formula: 5 × (C+N) min, 0.70 max. Si max 0.75 (not 1.00).

A worked example shows how the formula is checked. If a heat reports C = 0.05% and N = 0.04%, then C+N = 0.09%, the titanium minimum is 5 × 0.09 = 0.45%, and the maximum stays at 0.70%, so a reported Ti of 0.50% passes while 0.40% fails. Both carbon and nitrogen must therefore appear on the MTC, and receiving inspection should do the calculation rather than simply checking that some titanium is present. Nitrogen ≤0.10% is a maximum here, unlike ASME SA312 TP316N Stainless Steel Pipe, where nitrogen is an intentional 0.10–0.16% band.

Compared with ASME SA312 TP316L Stainless Steel Pipe, which caps carbon at 0.035% and has no titanium, TP316Ti allows up to 0.08% carbon because titanium ties it up. Compared with ASME SA312 TP321 Stainless Steel Pipe, TP316Ti keeps molybdenum at 2–3%. Compared with ASME SA312 UNS S31272 Stainless Steel Pipe, which uses a fixed Ti 0.30–0.60% range plus boron, TP316Ti uses the formula. For product analysis, titanium uses the A480 band of 0.05 over near the 0.70% maximum, while the minimum stays tied to the heat C+N, so state that basis on the purchase order when product analysis is ordered.

Mechanical Properties of SA312 TP316Ti

Room-temperature tensile requirements for TP316Ti come from SA-312 Table 4 and are summarized below. These are minimum release values for the lot, not typical values, and design allowables must always be taken from the governing code tables for UNS S31635 rather than from a neighbouring grade.

Property TP316Ti
Tensile, min 75 ksi [515 MPa]
Yield, min 30 ksi [205 MPa]
Elongation 35% L / 25% T
Grain size No Table 5 requirement

Room-temperature floors of 75/30 ksi match ASME SA312 TP316 Stainless Steel Pipe. Table 4 does not set a hardness maximum, and TP316Ti has no Table 5 grain-size requirement. Elevated-temperature design must use the code allowable stresses listed for UNS S31635; borrowing ASME SA312 TP316H Stainless Steel Pipe rows is not appropriate unless the pipe also carries genuine H-grade evidence, which TP316Ti does not require.

Certificate values are normally above the minima, but design should still use Table 4 and the code tables unless the mill has accepted higher guaranteed values in writing. Delivery is the solution-annealed condition. If EN 1.4571 dual certification is ordered, check both standards’ tensile floors and elongation rules, because the mill must satisfy the stricter value in each case.

Dimensions and Tolerances

Dimensional supply for SA312 TP316Ti pipe follows ASME B36.19 schedules for the common NPS and schedule combinations, with special OD and wall available by agreement when a project needs a section the schedules do not cover. Outside-diameter variations follow ASTM A999/A999M, and wall-thickness variations follow SA-312 Table 3 as summarized below. State on the purchase order whether wall is nominal or minimum (Supplementary S8), because the two readings produce different pipe from the same size line.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

Source: SA-312 Table 3; outside diameter variations per A999/A999M.

  • Lengths — single random, double random, or cut-to-length on order
  • Cut lengths — typically no more than 1/4 in. [6 mm] over the ordered length unless the PO states a tighter band
  • Ends — plain or beveled; confirm bevel angle and root face when the WPS is already frozen

Many chemical-process and industrial buyers order by OD × wall rather than NPS and schedule, which is fine as long as the enquiry says so clearly. Straightness, end finish, and length tolerance should be written into export orders so receiving inspection has an agreed acceptance basis instead of arguing after arrival. On thin schedules with threaded or socket-weld ends, check that the remaining wall is still adequate after the 12.5% under-tolerance. Jointers are not permitted unless the purchase order allows them, so cut-to-length programmes should include an allowance for fit-up scrap rather than expecting the mill to ship short pieces.

Equivalent Grades

TP316Ti / UNS S31635 is closely related to EN 1.4571 and to 316Ti trade designations, which makes it one of the easier SA-312 grades to cross-reference. The table below shows the practical maps and what to recheck.

Designation Notes
SA-312 TP316Ti / S31635 Governing
316Ti trade / EN 1.4571 maps Recheck Ti formula, Si ≤0.75, Mo

Equivalence is not automatic. EN 1.4571 uses a titanium formula based on carbon alone in many editions and may allow a different silicon limit, so a heat certified only to EN can miss the SA-312 5 × (C+N) minimum or the Si ≤0.75% cap. Dual certification is valid only when every Table 1 limit and the 75/30 ksi floor are met. Related SA-312 pages: ASME SA312 TP316 Stainless Steel Pipe, ASME SA312 TP316L Stainless Steel Pipe, ASME SA312 TP316H Stainless Steel Pipe, ASME SA312 TP321 Stainless Steel Pipe, and ASME SA312 UNS S31272 Stainless Steel Pipe.

Heat Treatment and Delivery Condition

TP316Ti is not individually listed in Table 2, so the default solution anneal at 1900 °F [1040 °C] minimum applies, followed by rapid cooling in water or by other rapid means. The anneal dissolves chromium carbides formed during hot working while leaving titanium carbonitrides in place, and rapid cooling prevents carbides from reforming as the pipe passes through the sensitizing range. The MTC should state the actual anneal temperature and the cooling method.

TP316Ti is not an H grade, so there is no clause 6.2 reheat, no Table 5 grain-size rule, and no mandatory clause 17 lot marking. Some owners order a separate stabilizing heat treatment for service in the sensitizing range; if so, it must be written into the purchase order and must not be confused with or replace the mandatory solution anneal. Bright annealing is available by agreement where the mill can hold temperature in a protective atmosphere.

Corrosion Resistance

SA-312 does not contain a corrosion table, so this section is engineering commentary. TP316Ti has the same Cr, Ni, and Mo as the rest of the 316 family, so its pitting and general corrosion resistance at ambient temperature is broadly similar to TP316. Its advantage is stability against intergranular corrosion after welding or exposure in the sensitizing range, which allows it to carry a higher carbon limit than TP316L while still resisting weld decay.

  • Intergranular corrosion — titanium stabilization helps; S7 (A262 Practice E) can be ordered when proof is needed
  • Chloride pitting — similar to TP316 thanks to Mo 2–3%
  • Knife-line attack — a narrow zone next to the fusion line can still be attacked in some strong oxidizing acids; review weld procedure and service with the materials engineer
  • Chloride stress corrosion cracking — similar susceptibility to other 300-series grades

Titanium-rich inclusions can affect polishability and, in a few very clean services, surface performance, so for polished or hygienic finishes discuss whether ASME SA312 TP316L Stainless Steel Pipe would be the better choice. For aggressive chloride duties beyond the 316 family, step up to a higher-Mo grade rather than relying on stabilization.

Applications of SA312 TP316Ti Pipe

Applications for TP316Ti pipe combine moderate chloride resistance with stability during welding or service in the sensitizing range. The table below summarizes where buyers typically specify the grade.

Application Why Note
Welded process lines needing Mo + stabilization Ti + Mo 2–3% Prove Ti ≥5×(C+N)
Chemical plants replacing 316L where C creeps up Stabilization Compare 316L economics

Typical users include chemical and petrochemical plants, heat exchangers, process lines operating in the sensitizing range, and European-designed plant built to 1.4571 practice and procured to ASME. Enquiries should state whether EN dual marking is needed, whether S7 testing applies, and the filler basis. When welding is the only concern and service temperatures are low, ASME SA312 TP316L Stainless Steel Pipe is often cheaper and easier to source.

Weldability

Table 6 in the extracted edition does not assign an AWS filler class to TP316Ti, so the consumable is by agreement and must be named on the WPS. Industry practice is either a 316-type low-carbon filler or a niobium-stabilized 318-type filler, because titanium transfers poorly across the arc and a titanium-bearing wire does not reliably produce a stabilized deposit. The choice is a project decision, not a Table 6 mandate, so record it on the WPS and PQR and qualify it on TP316Ti base metal.

  • Qualify on TP316Ti — procedure qualification on the actual grade
  • Control heat input — to limit the zone exposed to the sensitizing range
  • Back-purge roots — to protect the ID from oxidation
  • Clean after welding — pickle or remove heat tint where the owner specification requires it

Mill longitudinal welds on WLD and HCW pipe are made without filler, so the filler question applies only to fabrication joints. NDE extent for girth welds is a fabrication-code decision, separate from the hydro or electric test the mill applies to each length. Passivation after extensive field welding should follow the owner’s chemical-cleaning specification and rinse criteria.

Surface Finishes

Surface condition for SA312 TP316Ti pipe should be stated on the purchase order rather than left to mill default. For stainless pipe, embedded free iron, residual scale, and chloride-bearing residues are where corrosion starts, so the finish is part of the material performance and not just appearance. The finishes we regularly quote for this grade are listed below.

  • Annealed and pickled (AP) — solution annealed at 1900 °F [1040 °C] minimum, then descaled in acid pickle or an equivalent process to a matte grey finish; the standard choice for process pipe
  • Blasted and pickled — common on heavy-wall seamless where blasting first makes scale removal more reliable
  • Bright annealed (BA) — annealed in a protective atmosphere where mill capability exists for the size; the anneal temperature still has to meet the Table 2 practice for TP316Ti
  • Mechanically polished — OD and/or ID polish to an agreed grit or Ra when ordered; polishing never replaces the solution anneal
  • Bead-finished welded OD — weld bead rolled or ground flush as agreed on WLD and HCW product

For TP316Ti, titanium-rich inclusions can show up as streaks on highly polished surfaces, so agree the finish standard in advance if appearance or cleanability matters. Passivation after pickling or polishing can be added when the end-user specification calls for it, even though SA-312 itself does not require it. If the project bans chloride-bearing marking inks, say so on the order; otherwise the mill will apply its normal stencil practice and ship its default AP finish.

Inspection and Testing

The base acceptance package for SA-312 TP316Ti pipe combines chemistry, tensile testing, heat-treatment evidence, and a pressure or electrical integrity test on every length. The items below make up the usual package; supplementary requirements and project corrosion tests only apply when they are written on the purchase order.

  • Heat (melting) analysis — mandatory per heat against Table 1 for TP316Ti: C ≤0.08%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤0.75%, Cr 16.0–18.0%, Ni 10.0–14.0%, Mo 2.00–3.00%, N ≤0.10%, and Ti 5 × (C+N) minimum, 0.70% maximum
  • Product analysis — when ordered (Suppl. S1 or PO wording), using A480 Table A1.1 tolerances via A999 §6.3; product Ti maximum uses the A480 0.05 over band, minimum tied to heat C+N
  • Tension test — 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield minimum, plus 35% L / 25% T elongation on a lot basis
  • Flattening test — or the alternate bend test where the standard permits
  • Hydrostatic or nondestructive electric test — every length; manufacturer’s option unless the order fixes the method
  • Visual and dimensional check — against ordered NPS/schedule or OD × wall, with TP316Ti (UNS S31635) on every stencil

Mill test certificates: EN 10204 3.1 is the standard documentation from SHH STEEL supply. For TP316Ti the certificate must report the full Table 1 chemistry with C, N, and Ti as actual values so the 5 × (C+N) minimum and 0.70% maximum can be checked, together with Si ≤0.75%, 75/30 ksi tensile results, 35%/25% elongation, the hydro or NDE method, and the 1900 °F anneal statement. EN 10204 3.2 or third-party witness by SGS, Bureau Veritas, TÜV, or the buyer’s nominated agency is arranged when specified, and it should be booked before final testing rather than after the heat has been released. Dual ASME SA-312 / ASTM A312 certification is available when chemistry, heat treatment, mechanical tests, and marking satisfy both editions named on the order.

Option Purpose
S1 product analysis Confirms chemistry on finished pipe
S5 radiography Weld integrity on WLD pipe
S7 intergranular corrosion A262 Practice E after sensitizing treatment
S8 minimum wall Wall interpreted as minimum rather than nominal
S9 weld decay Compares weld and base-metal loss rates

Receiving review should calculate 5 × (C+N) from the MTC and compare it with the reported titanium, then check Ti ≤0.70%, Si ≤0.75%, Mo 2.00–3.00%, N ≤0.10%, the 75/30 ksi results, elongation, and the anneal statement. Third-party inspectors should check that the stencil reads TP316Ti and not only TP316. PMI that reports titanium is a useful check when TP316Ti shares a laydown area with TP316L or TP321.

Packaging and Shipping

Export and domestic shipments of SA312 TP316Ti pipe are packed for handling and for ocean or land transport. The packing we normally apply is summarized below, and anything beyond it can be agreed on the order.

  • Seaworthy bundles — pipes strapped or cradled in bundles sized for container or break-bulk handling, with non-metallic separators where the finish needs protecting
  • End caps — plastic or metal caps on plain or beveled ends to keep out damage and contamination in transit
  • Marking — specification, grade (TP316Ti (UNS S31635)), heat number, size, manufacturing type (SML / WLD / HCW), test letters, and mill identity as SA-312 and the purchase order require
  • Export protection — waterproof wrapping or desiccant as agreed for polished or bright-annealed finishes, with low-chloride inks on request

Segregate TP316Ti from ASME SA312 TP316L Stainless Steel Pipe, ASME SA312 TP316 Stainless Steel Pipe, and ASME SA312 TP321 Stainless Steel Pipe on the packing list and in the yard, because the grades look identical. Use separate bundles and distinct tags on mixed shipments, and have receiving inspectors check stencil heat numbers against the MTC for every length. Keep interiors dry and capped so chloride-bearing moisture cannot stain or pit the surface before installation. Shipping documents normally include the packing list, invoice, bill of lading or air waybill, and the 3.1 or 3.2 MTC with full Table 1 chemistry, plus origin and customs papers to suit the agreed Incoterms.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless plate and pipe, and for SA312 TP316Ti we quote against the edition you name rather than a generic catalogue sheet. We report the full Table 1 chemistry on the MTC with carbon, nitrogen, and titanium as actual values so the 5 × (C+N) ratio can be verified, together with the Si ≤0.75% result, the 75/30 ksi Table 4 results, and the 1900 °F anneal statement. Heat identity stays unbroken from the melt to the finished length, so receiving inspection can clear each heat against Table 1 and Table 4 without chasing paperwork after the pipe has arrived.

We check supplier certificates before shipment for missing nitrogen values, titanium below the calculated minimum, silicon above 0.75%, and EN-only certificates presented as ASME, so problems are caught at the mill. We are also open about what the standard does not specify: Table 6 assigns no filler class, and EN 1.4571 is a close map rather than an automatic equivalent.

  • Specification fidelity — chemistry and tensile to SA-312/A312 Table 1 and Table 4 for TP316Ti; C, N, and Ti reported with 5 × (C+N) check; Si ≤0.75%; 75/30 ksi confirmed; 1900 °F anneal stated
  • Mill resources — SML, WLD, and HCW from qualified stainless pipe mills with heat traceability; cutting and beveling on confirmed orders
  • Documentation — EN 10204 3.1 MTCs as standard with full Table 1 chemistry; 3.2 or third-party inspection on request
  • Dual marking — ASME SA-312 and ASTM A312 when the heat and tests meet both editions you name
  • Related grades — ASME SA312 TP316L Stainless Steel Pipe, ASME SA312 TP316 Stainless Steel Pipe, ASME SA312 TP316H Stainless Steel Pipe, and ASME SA312 TP321 Stainless Steel Pipe when a project buys a matched package
  • Export packing — seaworthy bundles, end protectors, and durable grade, heat, size, and type marking

Quotations follow your purchase-order language for edition year, manufacturing type, size, wall, finish, and any supplementary tests you name (S1, S5, S7, S8, S9). If the same project also needs plate or fittings, ask for coordinated heats so the chemistry lines up across product forms. Grade hub: ASME SA 312/SA 312M.

Supply Capability

SHH STEEL can supply ASME SA312 TP316Ti stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade.

Item SHH STEEL capability for TP316Ti
Standard ASME SA-312/SA-312M and/or ASTM A312/A312M TP316Ti / UNS S31635
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD/wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length SRL, DRL, or cut-to-length
Finish Annealed and pickled; blasted and pickled; bright annealed or polished by agreement
Testing Tension (75/30 ksi), flattening/bend, hydro or NDE per length; C, N, and Ti on MTC with 5 × (C+N) check; 1900 °F anneal stated; S1/S5/S7/S8/S9 on order
Documents EN 10204 3.1 with full Table 1 chemistry; third-party inspection / 3.2 on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

Common TP316Ti sizes are sometimes available from stock, especially material dual-certified with EN 1.4571, but check that the certificate shows C, N, and Ti and meets SA-312. Heavy-wall seamless and special sizes are usually mill-order items. Enquiries should state the SA-312 edition, TP316Ti (UNS S31635), SML/WLD/HCW, NPS or OD × wall (and whether wall is nominal or minimum), length practice, finish, and any product-analysis, corrosion-test, or 3.2 requirements, so mill slots line up with your need date. Cut lengths, beveling, and packing-list marking are available on confirmed orders, and grouping project sizes onto one heat keeps the chemistry consistent while helping meet mill minimums without over-ordering.

FAQ

Is ASME SA312 the same as ASTM A312 for TP316Ti?
For chemistry (Table 1), tensile (Table 4), manufacturing types, and most testing language, ASME SA-312/SA-312M matches ASTM A312/A312M of the referenced edition, and TP316Ti has the same row in both. Dual SA312/A312 marking is common when ordered. Name both editions on the purchase order and the mill test certificate so inspectors can verify the heat against the books you cited.
What is the UNS number for TP316Ti?
Table 1 lists TP316Ti as UNS S31635. Cite both TP316Ti and S31635 on the purchase order, the stencil, and the mill test certificate. Keeping the UNS on every document stops the pipe being confused with TP316 (S31600) or TP316L (S31603), which share the same Cr, Ni, and Mo ranges but have no titanium requirement.
TP316Ti vs TP316L — which should I order?
TP316L controls weld sensitization by keeping carbon at 0.035% or below and has a 70/25 ksi floor. TP316Ti allows carbon up to 0.08% and ties it up with titanium at 5 × (C+N) minimum, with a 75/30 ksi floor. TP316Ti suits service in the sensitizing range, while TP316L is usually cheaper and easier to polish for lower-temperature duty.
TP316Ti vs TP321 — which should I order?
Both are titanium-stabilized, but TP321 is an 18-8 grade with no molybdenum requirement, while TP316Ti keeps Mo 2.00–3.00% for better chloride pitting resistance. Choose TP316Ti when the process contains chlorides or reducing acids that benefit from molybdenum, and TP321 when stabilization is the only requirement and cost matters.
Seamless vs welded TP316Ti — which is better?
Neither is universally better. Seamless is typical for higher-pressure lines and heavy walls, while WLD and HCW are economical in larger diameters and thinner walls when tested and annealed to SA-312. Choose the route your design code and datasheet allow, and confirm the same SML, WLD, or HCW letters on the marking and MTC.
Can you dual-certify SA312 / A312 TP316Ti and EN 1.4571?
SA312/A312 dual marking is straightforward when the heat and tests meet both editions named on the order. EN 1.4571 dual certification is also common but needs care, because the EN titanium formula and silicon limit can differ from SA-312. The heat must satisfy 5 × (C+N) minimum titanium, Si ≤0.75%, and the 75/30 ksi floor as well as the EN requirements.
Hydrostatic test vs NDE — which do I get on TP316Ti pipe?
Each length is either hydrostatically tested or nondestructively electrically tested, and the manufacturer may choose unless the purchase order fixes the method. If your piping class or client specification requires one, state it on the PO and confirm the chosen test on the MTC for every length. NPS 10 and larger may be marked NH only when you accept a system test.
What heat treatment applies to TP316Ti?
TP316Ti is not individually listed in Table 2, so the default solution anneal at 1900 °F [1040 °C] minimum applies, followed by rapid cooling. It is not an H grade, so there is no clause 6.2 reheat or Table 5 grain-size requirement. A stabilizing heat treatment is a project extra and must never replace the mandatory solution anneal.
What Table 1 chemistry defines TP316Ti?
Table 1 sets C ≤0.08%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤0.75%, Cr 16.0–18.0%, Ni 10.0–14.0%, Mo 2.00–3.00%, N ≤0.10%, and Ti 5 × (C+N) minimum with 0.70% maximum. Silicon is tighter than the 1.00% of most 316 grades, and both C and N must be reported to prove the titanium ratio.
What are the Table 4 tensile requirements for TP316Ti?
Table 4 requires 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield minimum, with 35% longitudinal and 25% transverse elongation, the same floors as TP316. There is no Table 5 grain-size requirement. Elevated-temperature design should use the code allowables listed for UNS S31635 rather than TP316H rows.
What filler metal should I use to weld TP316Ti pipe?
Table 6 in the extracted edition assigns no AWS class to TP316Ti, so filler is by agreement. Common practice is a 316L-type or niobium-stabilized 318-type consumable, since titanium transfers poorly across the arc. Name the chosen consumable on the WPS and PQR and qualify it on TP316Ti base metal before production welding.
How much titanium does TP316Ti need?
Titanium must be at least 5 × (C+N) and no more than 0.70%. For example, a heat with C 0.05% and N 0.04% needs Ti of at least 0.45%. Because the minimum changes with each heat, receiving inspection should calculate it from the reported carbon and nitrogen rather than accepting any titanium value that simply appears on the MTC.

Conclusion

ASME SA312 TP316Ti / UNS S31635 is the titanium-stabilized 316 pipe grade, with C ≤0.08%, Si ≤0.75%, Cr 16.0–18.0%, Ni 10.0–14.0%, Mo 2.00–3.00%, N ≤0.10%, and Ti 5 × (C+N) minimum to 0.70% maximum, a 75/30 ksi Table 4 floor with 35% L / 25% T elongation, and the 1900 °F [1040 °C] default anneal. It is not an H grade, and Table 6 assigns no filler class, so the consumable is by agreement. It is not a drop-in for ASME SA312 TP316L Stainless Steel Pipe, ASME SA312 TP321 Stainless Steel Pipe, or ASME SA312 UNS S31272 Stainless Steel Pipe. Order the manufacturing type, size and wall, finish, C/N/Ti reporting, anneal proof, filler basis, any EN 1.4571 dual marking, and supplementary tests explicitly. For stock checks, mill certificates, or dual SA-312/A312 supply questions, contact SHH STEEL at admin@steelspecs.com or browse the ASME SA 312/SA 312M category on steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X