ASME SA312 TP304LN Stainless Steel Pipe | ASME SA312 Stainless Steel - SHH STEEL

ASME SA312 TP304LN Stainless Steel Pipe | SA 312/SA 312M

ASME SA312 TP304LN / UNS S30453 low-carbon nitrogen stainless steel pipe in SML, WLD and HCW, with C ≤0.035% and N 0.10–0.16%, a 75/30 ksi Table 4 floor and a 1900 °F solution anneal, supplied by SHH STEEL with EN 10204 3.1 MTCs for nuclear, cryogenic and chemical service.
Grade
TP304LN / UNS S30453
Standard
ASME SA312 / SA 312M (ASTM A312 / A312M)
Product form
Seamless (SML), welded (WLD), and heavily cold-worked (HCW) stainless steel pipe
Outside diameter
ASME B36.19 schedules (commonly Sch 5S / 10S / 40S / 80S) and special OD/wall by agreement; typical NPS from 1/8 upward (confirm on enquiry)
Share:
Overview
Manufacturing Types
Chemical Composition
Mechanical Properties
Dimensions
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ASME SA312 TP304LN Stainless Steel Pipe

ASME SA-312/SA-312M covers seamless, welded, and heavily cold-worked austenitic stainless steel pipe for high-temperature and general corrosive service, and it is the ASME Code adoption of ASTM A312/A312M. TP304LN / UNS S30453 combines two modifications of basic 18-8 stainless: the low carbon of ASME SA312 TP304L Stainless Steel Pipe and the controlled nitrogen of ASME SA312 TP304N Stainless Steel Pipe. Lowering carbon protects welded joints from sensitization but costs strength, and adding nitrogen gives that strength back without forming grain-boundary carbides, so designers get TP304 allowables with TP304L weld behaviour in a single grade.

Table 1 sets C ≤0.035%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 18.0–20.0%, Ni 8.0–12.0%, and N 0.10–0.16%. Footnote D, the 0.040% carbon allowance for small tubes, applies to TP304L and TP316L only, not to TP304LN. Table 4 sets 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield minimum with 35% longitudinal / 25% transverse elongation, the same floors as ASME SA312 TP304 Stainless Steel Pipe. TP304LN is not individually listed in Table 2, so the default 1900 °F [1040 °C] anneal applies, and Table 6 lists ER308L as the filler. The grade is closely associated with nuclear-plant piping and cryogenic equipment.

SHH STEEL can supply ASME SA312 TP304LN stainless steel pipe to the edition named on the enquiry, in seamless (SML), welded (WLD), and heavily cold-worked (HCW) form. We quote ASME B36.19 schedules and special OD/wall by agreement, ship with EN 10204 3.1 mill test certificates reporting carbon against the 0.035% ceiling, nitrogen inside 0.10–0.16%, and the 75/30 ksi results, and offer dual SA-312/A312 marking and, where the heat qualifies, dual grades such as TP304L/TP304LN. Please confirm NPS, wall or schedule, finish, owner restrictions such as ferrite or cobalt limits, and supplementary tests when you enquire.

The names below are the ones buyers commonly use, and they map to the ordered product as shown. Put both TP304LN and S30453 on the order, because the low-carbon and nitrogen requirements are both invisible on the pipe and only the certificate proves them.

  • ASME SA312 TP304LN / UNS S30453 — preferred marking language for ASME-code and dual-marked pipe
  • ASTM A312 TP304LN — same grade tables when the ASTM edition is referenced
  • “304LN” pipe — common shorthand; the certificate must show both the carbon ceiling and the nitrogen band
  • EN 1.4311 / JIS SUS304LN — commonly cited regional equivalents, approximate only

Sister grades buyers compare with TP304LN include ASME SA312 TP304L Stainless Steel Pipe (same low carbon without nitrogen, 70/25 ksi), ASME SA312 TP304N Stainless Steel Pipe (same nitrogen with C ≤0.08%, 80/35 ksi), ASME SA312 TP304 Stainless Steel Pipe, and ASME SA312 TP316LN Stainless Steel Pipe when molybdenum is also needed. Grade hub: ASME SA 312/SA 312M.

Manufacturing Types (SML / WLD / HCW)

ASME SA-312 recognizes three manufacturing routes for TP304LN pipe, and the route is a purchase-order decision driven by the design code, the size range, wall thickness, and how the owner wants the pipe inspected. The route never changes the chemistry: whichever way the pipe is made, the heat must still meet C ≤0.035%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 18.0–20.0%, Ni 8.0–12.0%, and N 0.10–0.16%, and every length must still go through the solution anneal at 1900 °F [1040 °C] minimum before it is released.

  • Seamless (SML) — no welding at any stage. Seamless is typical for nuclear and other high-integrity piping, heavy walls, and classes written around seamless product; it still has to be solution annealed before release.
  • Welded (WLD) — automatic welding without filler metal, with the weld finished so the pipe meets dimensional and mechanical requirements after the final heat treatment. The strip or plate heat must itself carry the full TP304LN chemistry, so ask for the coil or plate heat number on the certificate.
  • Heavily cold-worked (HCW) — welded pipe cold worked to at least 35% reduction of wall and weld before the final anneal, again without filler in the longitudinal seam, with the weld radiographed before cold work. Order HCW when the project specifically wants that marking and the process controls SA-312 writes around it.

Every finished length is hydrostatically tested or nondestructively electrically tested, and the mill may choose the method unless the purchase order fixes one. Pipe NPS 10 and larger may ship marked “NH” only when the purchaser accepts a system test in place of the hydrotest, and lots for mechanical testing follow clause 11.1. Owner specifications for nuclear or cryogenic service often add requirements beyond SA-312, such as ferrite limits or extra NDE, so put them on the purchase order rather than expecting the mill to infer them. Check the SML, WLD, or HCW letters and the hydro or NDE method on the certificate when comparing offers.

TP304LN is a specialist grade that is rarely stocked in depth, so most orders are planned mill runs, and seamless sizes may carry minimum quantities. Give us the route, sizes, wall, edition year, owner restrictions, and need date early, and we will tell you honestly what lead time and heat grouping are realistic for the package.

Chemical Composition of SA312 TP304LN

Two chemistry layers matter for TP304LN. The melting (heat or ladle) analysis is mandatory for every heat under SA-312/A312 Table 1, while product analysis on finished pipe applies only when it is ordered through Supplementary Requirement S1 or purchase-order wording. Product tolerances are not printed in SA-312 itself; they come through ASTM A999/A999M §6.3 from ASTM A480/A480M Table A1.1. SHH STEEL reports the actual ladle values and, when ordered, the product values, and never quotes tighter catalogue windows that the standard does not publish.

The tables below reproduce the Table 1 heat analysis for TP304LN and the product-analysis limits that result from applying the A480 Table A1.1 tolerances. Values are maximum unless a range is shown, and an ellipsis (…) means the ordered edition sets no requirement for that element, so it need not be reported.

Melting analysis (heat / ladle analysis) — Table 1

Element TP304LN (UNS S30453) melting analysis
Carbon (C) ≤ 0.035
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.030
Silicon (Si) ≤ 1.00
Chromium (Cr) 18.0 – 20.0
Nickel (Ni) 8.0 – 12.0
Nitrogen (N) 0.10 – 0.16
Molybdenum (Mo) … (no requirement)

Product analysis — A480/A480M Table A1.1 tolerances applied to Table 1

Element Melting (Table 1) Tolerance (A480 A1.1) Product analysis limit
Carbon (C) ≤ 0.035 0.01 over ≤ 0.045
Manganese (Mn) ≤ 2.00 0.04 over ≤ 2.04
Phosphorus (P) ≤ 0.045 0.010 over ≤ 0.055
Sulfur (S) ≤ 0.030 0.005 over ≤ 0.035
Silicon (Si) ≤ 1.00 0.05 over ≤ 1.05
Chromium (Cr) 18.0 – 20.0 0.20 under / over 17.80 – 20.20
Nickel (Ni) 8.0 – 12.0 0.10 under / 0.15 over 7.90 – 12.15
Nitrogen (N) 0.10 – 0.16 0.01 under / over 0.09 – 0.17
Element TP304L (S30403) TP304N (S30451) TP304LN (S30453)
C ≤ 0.035 ≤ 0.08 ≤ 0.035
Ni 8.0 – 13.0 8.0 – 11.0 8.0 – 12.0
N … 0.10 – 0.16 0.10 – 0.16
Tensile / yield min, ksi 70 / 25 80 / 35 75 / 30

Two values define TP304LN and both must be checked on receipt: carbon at or below 0.035% and nitrogen inside 0.10–0.16%. Nickel runs 8.0–12.0%, between the 8.0–11.0% of ASME SA312 TP304N Stainless Steel Pipe and the 8.0–13.0% of ASME SA312 TP304L Stainless Steel Pipe, giving the mill room to balance the austenite once carbon has been removed. Because Footnote D does not apply to this grade, the 0.035% carbon ceiling holds for every size, including small-OD and light-wall pipe.

On product analysis the finished pipe may read up to C 0.045%, Mn 2.04%, P 0.055%, S 0.035%, and Si 1.05%, with Cr 17.80–20.20%, Ni 7.90–12.15%, and N 0.09–0.17%. Nuclear and cryogenic owners frequently add their own restrictions on top of Table 1, so state any tighter carbon, cobalt, or ferrite requirement on the purchase order before the heat is selected rather than after the pipe is made.

Mechanical Properties of SA312 TP304LN

Room-temperature tensile requirements for TP304LN come from SA-312 Table 4 and are summarized below. These are minimum release values for the lot, not typical values, and design allowables must always be taken from the governing code tables for UNS S30453 rather than from a neighbouring grade.

Property (SA-312 Table 4) TP304LN
Tensile strength, min 75 ksi [515 MPa]
Yield strength (0.2% offset), min 30 ksi [205 MPa]
Elongation in 2 in. or 50 mm (or 4D), min 35% longitudinal / 25% transverse
Hardness No maximum listed in Table 4

The 75/30 ksi floor matches ASME SA312 TP304 Stainless Steel Pipe and sits above the 70/25 ksi of ASME SA312 TP304L Stainless Steel Pipe, which is the whole commercial case for the grade: nitrogen restores the strength the low carbon would otherwise cost. ASME SA312 TP304N Stainless Steel Pipe goes further to 80/35 ksi but keeps carbon at up to 0.08%. Table 4 lists no hardness maximum for TP304LN, so write any hardness limit on the purchase order if your fabrication needs one.

Whether TP304LN can replace TP304 without changing wall thickness depends on the code allowables listed for UNS S30453 in the governing edition, so the designer should check the tables rather than assume equality from the room-temperature floors. TP304LN is not an H grade and is not intended for creep-range design, where ASME SA312 TP304H Stainless Steel Pipe is the right family member.

Dimensions and Tolerances

Dimensional supply for SA312 TP304LN pipe follows ASME B36.19 schedules for the common NPS and schedule combinations, with special OD and wall available by agreement when a project needs a section the schedules do not cover. Outside-diameter variations follow ASTM A999/A999M, and wall-thickness variations follow SA-312 Table 3 as summarized below. State on the purchase order whether wall is nominal or minimum (Supplementary S8), because the two readings produce different pipe from the same size line.

NPS designator Wall over Wall under
1/8 to 2-1/2 incl., all t/D 20.0% 12.5%
3 to 18 incl., t/D up to 5% 22.5% 12.5%
3 to 18 incl., t/D over 5% 15.0% 12.5%
20 and larger, welded, all t/D 17.5% 12.5%
20 and larger, seamless, t/D up to 5% 22.5% 12.5%
20 and larger, seamless, t/D over 5% 15.0% 12.5%

Source: SA-312 Table 3; outside diameter variations per A999/A999M.

  • Lengths — single random, double random, or cut-to-length on order
  • Cut lengths — typically no more than 1/4 in. [6 mm] over the ordered length unless the PO states a tighter band
  • Ends — plain or beveled; confirm bevel angle and root face when the WPS is already frozen

Many nuclear, cryogenic, and chemical buyers order by OD × wall rather than NPS and schedule, which is fine as long as the enquiry says so clearly. Straightness, end finish, and length tolerance should be written into export orders so receiving inspection has an agreed acceptance basis instead of arguing after arrival. On thin schedules with threaded or socket-weld ends, check that the remaining wall is still adequate after the 12.5% under-tolerance. Jointers are not permitted unless the purchase order allows them, so cut-to-length programmes should include an allowance for fit-up scrap rather than expecting the mill to ship short pieces.

Equivalent Grades

TP304LN / UNS S30453 has commonly cited equivalents in European and Japanese standards, but nitrogen bands and strength floors may differ. Any cross-reference is a materials discussion, not a substitution approval for pressure-code pipe ordered to SA-312 or A312.

Designation Relationship to TP304LN
ASME SA-312 / ASTM A312 TP304LN Governing pipe grade
UNS S30453 Unified number in Table 1
ASME SA-240 / A240 304LN Plate counterpart (separate specification)
EN 1.4311 (X2CrNiN18-10) Commonly cited European low-carbon nitrogen-alloyed 304; verify in the EN standard
JIS SUS304LN Commonly cited Japanese counterpart; verify against JIS

EN 1.4311 and JIS SUS304LN are commonly cited approximate equivalents that were not verified against the EN or JIS texts for this page, and they do not authorize code substitution without engineered approval. Within SA-312, ASME SA312 TP304L Stainless Steel Pipe lacks the nitrogen and ASME SA312 TP304N Stainless Steel Pipe lacks the low carbon, so neither is a direct replacement. Related: ASME SA312 TP304 Stainless Steel Pipe and ASME SA312 TP316LN Stainless Steel Pipe.

Heat Treatment and Delivery Condition

All pipe furnished to SA-312 has to be heat treated. TP304LN is not individually listed in Table 2, so it takes the default solution anneal at 1900 °F [1040 °C] minimum, followed by water quenching or another rapid cool. The anneal dissolves any carbides and nitrides and restores the fully austenitic structure on which both the strength and the low-carbon corrosion behaviour rely, and the anneal statement belongs on the certificate for every lot.

Seamless pipe may be quenched directly after hot forming when the edition allows it and the finishing temperature is not below the minimum anneal; TP304LN is not an H grade, so the clause 6.2 reheat rule does not apply. HCW cold reduction is done before the final anneal, so delivery is always the annealed condition. Prolonged exposure in the nitride-precipitation range should be avoided in fabrication, and any post-forming re-anneal should follow the same 1900 °F minimum.

Corrosion Resistance

SA-312 has no corrosion table, so this section is engineering commentary rather than a specification requirement. TP304LN resists general corrosion like the rest of the 304 family, and its low carbon keeps welded joints free of the carbide networks that caused intergranular stress corrosion cracking in sensitized 304 welds in early nuclear plants. That history is the main reason nuclear owners moved toward low-carbon, nitrogen-controlled grades such as this one.

  • As-welded corrosion — low carbon protects the HAZ; S7 (A262 Practice E) can be ordered as proof
  • Chlorides and seawater — no molybdenum, so ASME SA312 TP316LN Stainless Steel Pipe or the 316 family is the better choice
  • Cryogenic duty — nitrogen helps keep the austenite stable at low temperature; confirm code acceptance for the service
  • Chloride stress corrosion cracking — similar susceptibility to other 300-series grades in warm chloride water

Deposits, stagnant pockets, and contamination remain the commonest cause of field failures, so drainage, cleanliness, and post-weld cleaning matter as much as chemistry. Site welds and ground areas should be cleaned and passivated when the end-user specification asks for it, and any owner water-chemistry or cleanliness rules should be passed to the fabricator together with the pipe.

Applications of SA312 TP304LN Pipe

Applications for TP304LN pipe come from combining TP304 strength with low-carbon weld behaviour and stable austenite. The table below summarizes where buyers typically specify the grade and what to check on the enquiry.

Application Why TP304LN Note
Nuclear plant piping and auxiliaries Low C for IGSCC resistance with TP304 strength Owner specs add tests and cleanliness rules
Cryogenic and LNG systems Nitrogen stabilizes austenite; low C helps welded joints Impact testing per code
Chemical plant welded lines Nitric acid and oxidizing media where weld decay is a concern Order S7 or S9
High-purity water and pharmaceutical utilities Weld-zone integrity and clean surfaces Specify finish and passivation
Pressure piping redesigned from 304 to low C Same strength floors as TP304 Use S30453 allowables
Heat exchangers and vessels Connection piping matching 304LN plate Plate and tube under separate specs

Typical users include nuclear power plants (auxiliary and recirculation-type piping where owners specify S30453), cryogenic and liquefied-gas equipment, and chemical plants that weld heavily and want TP304 allowables. Enquiries should state the design code, owner restrictions such as ferrite or cobalt, carbon and nitrogen reporting, and any dual marking. For chloride service see ASME SA312 TP316LN Stainless Steel Pipe.

Weldability

TP304LN welds by the same processes as ASME SA312 TP304L Stainless Steel Pipe and is chosen precisely so welded joints keep low-carbon corrosion behaviour. SA-312 Table 6 lists AWS A5.9 ER308L (UNS S30883 / W30843) as the filler, and ER308L should be recorded on the WPS and PQR so the deposit keeps the low carbon. The deposit does not carry the base-metal nitrogen, so where the design relies on full TP304LN strength across the joint, confirm weld-metal properties during qualification; owner ferrite limits for the weld metal should also be written into the procedure.

  • Qualify on TP304LN — with any owner ferrite or NDE requirements included
  • Control heat input and interpass temperature — to protect the HAZ and limit distortion
  • Back-purge roots — standard on nuclear and high-integrity lines
  • Clean joints — free of oil, paint, and carbon-steel contamination before welding

Mill longitudinal welds on WLD and HCW pipe are made without filler, so Table 6 applies to repairs and fabrication joints. Girth-weld NDE extent follows the piping or vessel code and the owner specification, separate from the hydro or electric test the mill applies to each length, and it should be agreed before fabrication starts.

Surface Finishes

Surface condition for SA312 TP304LN pipe should be stated on the purchase order rather than left to mill default. For stainless pipe, embedded free iron, residual scale, and chloride-bearing residues are where corrosion starts, so the finish is part of the material performance and not just appearance. The finishes we regularly quote for this grade are listed below.

  • Annealed and pickled (AP) — solution annealed at 1900 °F [1040 °C] minimum, then descaled in acid pickle or an equivalent process to a matte grey finish; the standard choice for process pipe
  • Blasted and pickled — common on heavy-wall seamless where blasting first makes scale removal more reliable
  • Bright annealed (BA) — annealed in a protective atmosphere where mill capability exists for the size; the anneal temperature still has to meet the Table 2 practice for TP304LN
  • Mechanically polished — OD and/or ID polish to an agreed grit or Ra when ordered; polishing never replaces the solution anneal
  • Bead-finished welded OD — weld bead rolled or ground flush as agreed on WLD and HCW product

For TP304LN the usual choice is annealed and pickled, and nuclear owners often add cleanliness and marking-ink restrictions that should be written on the order. Passivation after pickling or polishing can be added when the end-user specification calls for it, even though SA-312 itself does not require it. If the project bans chloride-bearing marking inks, say so on the order; otherwise the mill will apply its normal stencil practice and ship its default AP finish.

Inspection and Testing

The base acceptance package for SA-312 TP304LN pipe combines chemistry, tensile testing, heat-treatment evidence, and a pressure or electrical integrity test on every length. The items below make up the usual package; supplementary requirements and project corrosion tests only apply when they are written on the purchase order.

  • Heat (melting) analysis — mandatory per heat against Table 1 for TP304LN: C ≤0.035%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 18.0–20.0%, Ni 8.0–12.0%, and N 0.10–0.16%
  • Product analysis — when ordered (Suppl. S1 or PO wording), using A480 Table A1.1 tolerances via A999 §6.3
  • Tension test — 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield minimum, plus 35% L / 25% T elongation on a lot basis
  • Flattening test — or the alternate bend test where the standard permits
  • Hydrostatic or nondestructive electric test — every length; manufacturer’s option unless the order fixes the method
  • Visual and dimensional check — against ordered NPS/schedule or OD × wall, with TP304LN (UNS S30453) on every stencil

Mill test certificates: EN 10204 3.1 is the standard documentation from SHH STEEL supply. For TP304LN the certificate reports the full Table 1 chemistry with carbon shown against the 0.035% ceiling and nitrogen inside 0.10–0.16%, the 75/30 ksi tensile results with 35%/25% elongation, the hydro or NDE method, and the 1900 °F anneal statement. EN 10204 3.2 or third-party witness by SGS, Bureau Veritas, TÜV, or the buyer’s nominated agency is arranged when specified, and it should be booked before final testing rather than after the heat has been released. Dual ASME SA-312 / ASTM A312 certification is available when chemistry, heat treatment, mechanical tests, and marking satisfy both editions named on the order.

Option Purpose
S1 product analysis Confirms chemistry on finished pipe
S5 radiography Weld integrity on WLD pipe
S7 intergranular corrosion A262 Practice E after sensitizing treatment
S8 minimum wall Wall interpreted as minimum rather than nominal
S9 weld decay Compares weld and base-metal loss rates

Receiving review should confirm C ≤0.035%, N 0.10–0.16%, Cr 18.0–20.0%, Ni 8.0–12.0%, tensile at or above 75/30 ksi, the anneal statement, the test method, and any owner-specified extras, and that the stencil reads TP304LN rather than TP304L or TP304N. Handheld PMI guns cannot read carbon or nitrogen, so the certified analysis is the practical evidence of the grade.

Packaging and Shipping

Export and domestic shipments of SA312 TP304LN pipe are packed for handling and for ocean or land transport. The packing we normally apply is summarized below, and anything beyond it can be agreed on the order.

  • Seaworthy bundles — pipes strapped or cradled in bundles sized for container or break-bulk handling, with non-metallic separators where the finish needs protecting
  • End caps — plastic or metal caps on plain or beveled ends to keep out damage and contamination in transit
  • Marking — specification, grade (TP304LN (UNS S30453)), heat number, size, manufacturing type (SML / WLD / HCW), test letters, and mill identity as SA-312 and the purchase order require
  • Export protection — waterproof wrapping or desiccant as agreed for polished or bright-annealed finishes, with low-chloride inks on request

Segregate TP304LN from ASME SA312 TP304L Stainless Steel Pipe and ASME SA312 TP304N Stainless Steel Pipe on the packing list and in the yard, because these grades look identical and neither carbon nor nitrogen can be checked with a handheld PMI gun. Use separate bundles and distinct tags on mixed shipments, and have receiving check stencil heat numbers against the MTC. Keep interiors dry and capped so chloride-bearing moisture cannot stain or pit the surface before installation. Shipping documents normally include the packing list, invoice, bill of lading or air waybill, and the 3.1 or 3.2 MTC with full Table 1 chemistry, plus origin and customs papers to suit the agreed Incoterms.

Why Choose SHH STEEL

SHH STEEL supplies specification-driven stainless plate and pipe, and for SA312 TP304LN we quote against the edition you name rather than a generic catalogue sheet. We report the full Table 1 chemistry on the MTC with carbon against the 0.035% ceiling and nitrogen inside the 0.10–0.16% band, together with the 75/30 ksi results, and we quote against the edition you name. Heat identity stays unbroken from the melt to the finished length, so receiving inspection can clear each heat against Table 1 and Table 4 without chasing paperwork after the pipe has arrived.

The commonest problems we see with TP304LN are TP304L stock offered with residual nitrogen below 0.10%, certificates that omit nitrogen, and tensile results reported against the TP304L floor instead of 75/30 ksi. We check supplier certificates before shipment so those issues are caught at the mill rather than at the fabricator, and we pass owner restrictions to the mill before the heat is selected.

  • Specification fidelity — chemistry and tensile to SA-312/A312 Table 1 and Table 4 for TP304LN (S30453); C ≤0.035% and N 0.10–0.16% reported; 75/30 ksi verified; 1900 °F anneal stated
  • Mill resources — SML, WLD, and HCW from qualified stainless pipe mills with heat traceability; cutting and beveling on confirmed orders
  • Documentation — EN 10204 3.1 MTCs as standard with full Table 1 chemistry; 3.2 or third-party inspection on request
  • Dual marking — ASME SA-312 and ASTM A312 when the heat and tests meet both editions you name
  • Related grades — ASME SA312 TP304L Stainless Steel Pipe, ASME SA312 TP304N Stainless Steel Pipe, ASME SA312 TP304 Stainless Steel Pipe, and ASME SA312 TP316LN Stainless Steel Pipe when a project buys a matched package
  • Export packing — seaworthy bundles, end protectors, and durable grade, heat, size, and type marking

Quotations follow your purchase-order language for edition year, manufacturing type, size, wall, finish, and any supplementary tests you name (S1, S5, S7, S8, S9). If the same project also needs plate or fittings, ask for coordinated heats so the chemistry lines up across product forms. Grade hub: ASME SA 312/SA 312M.

Supply Capability

SHH STEEL can supply ASME SA312 TP304LN stainless steel pipe against the edition and manufacturing type named on your enquiry. The capability table below summarizes the routes, sizes, finishes, and documents we regularly quote for this grade.

Item SHH STEEL capability for TP304LN
Standard ASME SA-312/SA-312M and/or ASTM A312/A312M Grade TP304LN / UNS S30453
Manufacturing types SML, WLD, HCW
Size NPS 1/8 and up per ASME B36.19; special OD/wall by agreement
Schedules 5S, 10S, 40S, 80S and non-standard walls
Length SRL, DRL, or cut-to-length
Finish Annealed and pickled; blasted and pickled; bright annealed or polished by agreement
Testing Tension (75/30 ksi), flattening/bend, hydro or NDE per length; C ≤0.035% and N 0.10–0.16% reported on MTC; S1/S5/S7/S8/S9 on order
Documents EN 10204 3.1 with full Table 1 chemistry; third-party inspection / 3.2 on request
Trade terms FOB / CFR / CIF / EXW and other agreed Incoterms

TP304LN is rarely held in stock in depth, so most orders are mill runs grouped by heat. Tell us the full size list, owner restrictions, and need date early so mill slots can be matched, and we will be clear about lead time rather than promise stock that does not exist. Enquiries should state the SA-312 edition, TP304LN (UNS S30453), SML/WLD/HCW, NPS or OD × wall (and whether wall is nominal or minimum), length practice, finish, and any product-analysis, corrosion-test, or 3.2 requirements, so mill slots line up with your need date. Cut lengths, beveling, and packing-list marking are available on confirmed orders, and grouping project sizes onto one heat keeps the chemistry consistent while helping meet mill minimums without over-ordering.

FAQ

Is ASME SA312 the same as ASTM A312 for TP304LN?
For chemistry (Table 1), tensile (Table 4), manufacturing types, heat treatment, and most testing language, ASME SA-312/SA-312M matches ASTM A312/A312M of the referenced edition. Dual SA312/A312 marking is common when it is ordered. Name both editions on the purchase order and make sure the mill test certificate repeats them, so inspectors can verify the heat against the books you cited.
Seamless vs welded TP304LN — which is better?
Neither is universally better. Seamless is the usual choice for heavy walls, high-pressure lines, and piping classes written around seamless product, while WLD and HCW are fully legitimate SA-312 forms when they are tested and annealed to the standard and usually cost less in common sizes. Choose the route your design code and datasheet allow, and check that SML, WLD, or HCW appears on both the stencil and the MTC.
Hydrostatic test vs NDE — which do I get on TP304LN pipe?
Every length is either hydrostatically tested or nondestructively electrically tested, and the manufacturer may choose unless the purchase order fixes the method. If your piping class or client specification requires one of them, state it on the PO and confirm the chosen test on the MTC for each length. NPS 10 and larger may be marked NH only when you accept a system test instead.
Does SA-312 Table 4 set a hardness limit for TP304LN?
No. Table 4 lists tensile strength, yield strength, and elongation for TP304LN, but no hardness maximum, so catalogue Brinell or Rockwell figures are not specification requirements. If hardness matters for your fabrication or for an end-user rule, write the limit and the test method on the purchase order, and we will make sure the mill reports it on the certificate.
What is the UNS number and chemistry of TP304LN?
Table 1 lists TP304LN as UNS S30453 with C ≤0.035%, Mn ≤2.00%, P ≤0.045%, S ≤0.030%, Si ≤1.00%, Cr 18.0–20.0%, Ni 8.0–12.0%, and N 0.10–0.16%. Low carbon and the nitrogen band together define the grade. Put TP304LN and S30453 on every document so it is not confused with TP304L or TP304N.
How does TP304LN differ from TP304L?
Both limit carbon to 0.035%, but TP304LN also requires N 0.10–0.16%, which lifts the Table 4 floor to 75/30 ksi from the 70/25 ksi of TP304L, and its nickel window is 8.0–12.0% rather than 8.0–13.0%. Choose TP304LN when you want TP304 allowables with low-carbon weld behaviour in one grade.
How does TP304LN differ from TP304N?
Both require N 0.10–0.16%. TP304N allows carbon up to 0.08% and reaches an 80/35 ksi floor, while TP304LN limits carbon to 0.035% and has a 75/30 ksi floor. TP304LN is the better choice when welded joints must resist sensitization, and TP304N when maximum strength in the 304 family matters more to the design.
Does Footnote D (0.040% carbon for small tubes) apply to TP304LN?
No. In SA-312 Table 1, Footnote D applies to TP304L and TP316L only. TP304LN keeps the 0.035% carbon ceiling for every size, including small-OD and light-wall pipe, and the product-analysis limit is 0.045% with the A480 tolerance. Check the certificate carbon against 0.035% regardless of the pipe size.
Is TP304LN suitable for nuclear service?
TP304LN is widely associated with nuclear-plant piping, because its low carbon resists the intergranular stress corrosion cracking seen in sensitized 304 welds while nitrogen keeps TP304 strength. Nuclear orders usually carry owner and code requirements beyond SA-312, such as ferrite, cobalt, or extra NDE, so put every one of them on the purchase order.
Is TP304LN suitable for seawater or chloride service?
Not as a first choice. TP304LN has no molybdenum, so its pitting and crevice resistance in seawater, brine, or heavy chloride duty is limited, much like other 304-family grades. For chloride service look at TP316LN or the wider 316 family, and have the actual fluid, temperature, and crevice conditions reviewed by a corrosion engineer.
What filler and heat treatment apply to TP304LN?
SA-312 Table 6 lists ER308L (UNS S30883 / W30843) for TP304LN, and the grade takes the default Table 2 solution anneal at 1900 °F [1040 °C] minimum with rapid cooling. ER308L keeps the weld low in carbon, but the deposit does not carry the base-metal nitrogen, so confirm weld-metal properties when the design relies on full strength.

Conclusion

ASME SA312 TP304LN / UNS S30453 combines low carbon and controlled nitrogen, with C ≤0.035%, Cr 18.0–20.0%, Ni 8.0–12.0%, and N 0.10–0.16% in Table 1, a 75/30 ksi Table 4 floor with 35% L / 25% T elongation, the default 1900 °F [1040 °C] solution anneal, and ER308L filler from Table 6. It gives TP304 strength with ASME SA312 TP304L Stainless Steel Pipe weld behaviour, but it is neither the strongest 304 grade (ASME SA312 TP304N Stainless Steel Pipe) nor a chloride grade. Order the manufacturing type, size and wall, finish, carbon and nitrogen reporting, owner restrictions, and supplementary tests explicitly. For stock checks, mill certificates, or dual SA-312/A312 supply questions, contact SHH STEEL at admin@steelspecs.com or browse the ASME SA 312/SA 312M category on steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X