Q390MC TMCP Steel Plate GB/T 1591 Supplier
What is Q390MC TMCP Steel Plate GB/T 1591?
Q390MC, also searched as GB/T 1591 Q390MC, Q390MC steel plate, Q390MC TMCP plate and Q390 MC, is the 390 MPa quality-grade-C grade delivered by thermomechanical controlled process in GB/T 1591-2018. Q is the yield symbol, 390 is the thin-plate minimum yield in MPa, M is the delivery letter, and C is the quality letter for Charpy impact at 0°C.
The M is the point of this page. Normalized GB/T 1591 Q390NC has an N. A normalized certificate cannot be stamped MC. Grade B on the TMCP route is GB/T 1591 Q390MB. Normalized D is GB/T 1591 Q390ND. Normalized E is GB/T 1591 Q390NE. The 355 MPa TMCP sister at the same temperature is GB/T 1591 Q355MC. The full family sits on GB/T 1591. Do not drop a 390 MPa drawing onto a 355 MPa plate, and do not upgrade it to GB/T 1591 Q420NC without a price check.
EN 10025 has no S390 letter. The closest higher TMCP comparison is EN 10025-4 S420M, tested at −20°C. EN 10025-3 S420N is normalized. On the US side, ASTM A572 Gr.55 is 55 ksi / 380 MPa, one step lower, and it is not an MC twin. JIS G3106 SM520B is the usual Japanese comparison. Dual mark only when both books are fully met. See EN 10025-4 and high strength low alloy plates.
SHH STEEL is a global steel mill sourcing partner and steel manufacturer and exporter, mill-direct, China origin. We source Q390MC from first-line structural mills that can actually run the TMCP schedule, print heat analysis and product analysis when ordered, and ship plate to fabricators in the United States, Europe, the Middle East, Southeast Asia, Africa and South America. Related pages include structural steel plates and the products index.
Material Specification
| Specification Element | Requirement | SHH STEEL Compliance |
|---|---|---|
| Plate book | GB/T 1591-2018 Q390MC | Confirmed |
| Other search names | Q390MC steel plate, Q390 MC, Q390MC TMCP | Covered |
| Delivery condition | Thermomechanical controlled process | Confirmed |
| Yield, ≤ 16 mm | 390 MPa min | Confirmed |
| Quality grade | C, impact at 0°C | Confirmed |
| Not this page | Normalized GB/T 1591 Q390NC | Different condition |
| Warmer TMCP sister | GB/T 1591 Q390MB | +20°C |
| EN comparison | EN 10025-4 S420M is higher | Not a swap |
| US comparison | ASTM A572 Gr.55 is 380 MPa | Not a twin |
| Product analysis | GB/T 222 column when ordered | Confirmed |
| Supply role | Global steel mill sourcing partner | SHH STEEL |
| Certification | EN 10204 3.1 or 3.2 | As ordered |
Nearby pages that buyers compare, but must not swap blindly, include GB/T 1591 Q390NB, GB/T 1591 Q355MC and ASTM A572 Gr.55.
Chemical Composition
Heat analysis is the mill ladle table in GB/T 1591-2018 for TMCP Q390. Product analysis, when ordered, follows GB/T 222. Q390MC is a microalloyed HSLA plate. Grade C is tighter on phosphorus and sulfur than grade B, because the impact test is at 0°C. Mills may add Nb, V or Ti. The certificate shows the elements actually used. TMCP chemistry is often leaner than a normalized heat of the same yield, because the rolling schedule does part of the grain refinement.
Heat Analysis and Product Analysis — GB/T 1591 Q390MC, TMCP
| Element | Heat analysis (%) | Product analysis (%) |
|---|---|---|
| Carbon (C), max | 0.20 | 0.22 |
| Silicon (Si), max | 0.50 | 0.55 |
| Manganese (Mn), max | 1.70 | 1.80 |
| Phosphorus (P), max | 0.030 | 0.035 |
| Sulfur (S), max | 0.030 | 0.035 |
| Niobium (Nb), max | 0.07 | 0.08 |
| Vanadium (V), max | 0.20 | 0.22 |
| Titanium (Ti), max | 0.20 | 0.21 |
| Chromium (Cr), max | 0.30 | 0.35 |
| Nickel (Ni), max | 0.50 | 0.55 |
| Copper (Cu), max | 0.40 | 0.45 |
| Molybdenum (Mo), max | 0.10 | 0.11 |
| Nitrogen (N), max | 0.015 | 0.017 |
| Aluminium (Als), min when used | 0.015 | 0.010 |
Carbon equivalent is limited by thickness in the standard. The M route often has a lower CEV window than normalized GB/T 1591 Q390NC. If the purchase order writes product analysis, SHH STEEL prints both columns and the thickness band used for the tensile test. Do not treat this chemistry as quenched-and-tempered GB/T 16270 Q460C. A 355 MPa file is GB/T 1591 Q355C, not this grade.
Mechanical Properties
Buyers search Q390MC mechanical properties, Q390MC yield strength, GB/T 1591 Q390MC tensile and Q390MC impact 0°C.
Tensile and impact — GB/T 1591 Q390MC, TMCP
| Thickness | Yield min | Tensile | Elongation min | Impact |
|---|---|---|---|---|
| ≤ 16 mm | 390 MPa | 490–650 MPa | 20% | 0°C, grade C |
| > 16–40 mm | 380 MPa | 490–650 MPa | 20% | 0°C, grade C |
| > 40–63 mm | 360 MPa | 490–650 MPa | 19% | 0°C, grade C |
| > 63–80 mm | 350 MPa | 490–650 MPa | 19% | 0°C, grade C |
| > 80–100 mm | 340 MPa | 490–650 MPa | 19% | 0°C, grade C |
| > 100–150 mm | 330 MPa | 470–620 MPa | 18% | 0°C, grade C |
Impact energy is the average of three longitudinal Charpy V-notch specimens, commonly 34 J minimum at 0°C. One value may fall below the table, but not below 70% of that value. Write a higher energy on the order if the owner requires it.
Yield steps down with thickness. A 390 MPa name on 12 mm plate is not the minimum on a 40 mm flange. 390 MPa is about 56.5 ksi. ASTM A572 Gr.55 is 55 ksi and is not this book. SHH STEEL quotes the thickness band and the M condition on the offer.
Density is 7.85 g/cm³. Hardness is not a design value for this grade. Z15, Z25 or Z35 through-thickness tensile is an extra, not part of the C letter.
Material Comparison
| Grade | Book | Delivery | Yield, thin plate | Impact | Swap? |
|---|---|---|---|---|---|
| GB/T 1591 Q390NC | GB/T 1591-2018 | Normalized | 390 MPa | 0°C | Different process |
| GB/T 1591 Q390MB | GB/T 1591-2018 | TMCP | 390 MPa | +20°C | Warmer M sister |
| Q390MC | GB/T 1591-2018 | TMCP | 390 MPa | 0°C | This page |
| Q390MD | GB/T 1591-2018 | TMCP | 390 MPa | −20°C | Colder M sister |
| GB/T 1591 Q355MC | GB/T 1591-2018 | TMCP | 355 MPa | 0°C | Lower yield |
| GB/T 1591 Q420NC | GB/T 1591-2018 | Normalized | 420 MPa | 0°C | Higher yield |
| EN 10025-4 S420M | EN 10025-4 | TMCP | 420 MPa | −20°C | Higher comparison |
| ASTM A572 Gr.55 | ASTM A572 | As rolled | 380 MPa | Different | Lower yield |
A colder normalized file is GB/T 1591 Q390ND. A 460 MPa file is GB/T 1591 Q460D.
Equivalent Material Grades
There is no official one-to-one substitute for Q390MC. What buyers compare is a 390 MPa TMCP plate tested at 0°C.
EN 10025 has no S390. EN 10025-4 S420M is the higher TMCP comparison. EN 10025-3 S420N is normalized. EN 10025-2 S355JR is +20°C and only 355 MPa. In the United States, ASTM A572 Gr.55 is 55 ksi / 380 MPa. ASTM A572 Gr.50 is 50 ksi and is one step lower. ASTM A36 is 36 ksi and is well below this yield. In Japan, JIS G3106 SM520B is the usual comparison. SHH STEEL will not stamp EN 10025-4 S420M or ASTM A572 Gr.55 on a Q390MC certificate unless the purchase order names both books and both tables are met.
| Designation | Country / region | Standard | Notes |
|---|---|---|---|
| Q390MC | China | GB/T 1591-2018 | Name on this page |
| GB/T 1591 Q390NC | China | GB/T 1591-2018 | Normalized, not this page |
| GB/T 1591 Q390MB | China | GB/T 1591-2018 | TMCP, +20°C |
| GB/T 1591 Q355MC | China | GB/T 1591-2018 | 355 MPa, TMCP |
| GB/T 1591 Q420B | China | GB/T 1591-2018 | 420 MPa, hot rolled |
| EN 10025-4 S420M | Europe | EN 10025-4 | Higher TMCP comparison |
| ASTM A572 Gr.55 | USA | ASTM A572 | 55 ksi, lower yield |
| JIS G3106 SM520B | Japan | JIS G3106 | Usual Japanese comparison |
Structural Service
Buyers pick Q390MC when a building, bridge member or welded fabrication wants about 390 MPa yield, a TMCP condition, and impact at 0°C. Search phrases such as Q390MC steel plate and GB/T 1591 Q390MC all point here. The family index is GB/T 1591.
It is the wrong plate when the drawing says normalized. That work is GB/T 1591 Q390NC. It is the wrong plate for a +20°C file. That work is GB/T 1591 Q390MB, and the normalized sister is GB/T 1591 Q390NB. It is the wrong plate for a −20°C file. That work is Q390MD, and the normalized sister is GB/T 1591 Q390ND. It is the wrong plate for a −40°C file. That work is Q390ME, and the normalized sister is GB/T 1591 Q390NE. It is the wrong plate for a 355 MPa file. That work is GB/T 1591 Q355MC or GB/T 1591 Q355C. It is the wrong plate for a 420 MPa file. That work is GB/T 1591 Q420NC or GB/T 1591 Q420E. It is the wrong plate for a 460 MPa file. That work is GB/T 1591 Q460ND. It is the wrong plate for a pressure vessel. That work sits on ASTM A516 or pressure vessel steel plates.
SHH STEEL supplies this plate when the drawing names GB/T 1591, quality grade C, and the M condition at 390 MPa.
Weldability
Q390MC is a weldable TMCP HSLA structural plate. Carbon is controlled, and many heats use Nb, V or Ti. A procedure written for ASTM A36 is not a finished WPS for thick Q390MC. Carbon equivalent on the M route is often lower than normalized GB/T 1591 Q390NC, which helps the root pass, but the TMCP microstructure still needs a qualified procedure. A procedure qualified only at +20°C may miss the 0°C coupon.
Typical consumables are matching 55–60 ksi low-hydrogen electrodes or wires. E7018-class electrodes are under-matched if the joint must develop full plate strength. A procedure written for ASTM A572 Gr.55 is a useful strength reference after chemistry is checked. Preheat follows thickness, hydrogen and the approved WPS. Heat input should stay inside the mill window. A very high heat input can soften the TMCP zone next to the weld.
The fabricator owns the WPS. SHH STEEL can share mill heat data, product analysis and carbon equivalent for that review. Do not use a Q390MC procedure on GB/T 1591 Q355ME without checking the lower-yield carbon equivalent. Do not use it on GB/T 1591 Q460NE either.
Heat Treatment and Delivery Condition
Usual delivery from SHH STEEL for Q390MC is thermomechanical controlled process. The plate is not normalized as GB/T 1591 Q390NC.
TMCP combines controlled rolling and accelerated cooling. Finish rolling is held in the non-recrystallization range, then the plate is cooled on the run-out table to a finish temperature the mill records. Do not order Q390MC as quenched and tempered. That route belongs to GB/T 16270. Stress relief after fabrication, if used, should be agreed before cutting, because a high temper can move the TMCP properties.
The certificate lists GB/T 1591 Q390MC, heat number, delivery condition, heat analysis, product analysis when ordered, tensile by thickness band, and 0°C impact. Certificates may be EN 10204 3.1 or EN 10204 3.2. Dual marking to EN 10025-4 S420M is available only when both books are fully met.
Dimensions
Usual supply range from SHH STEEL for Q390MC steel plate:
- Thickness: commonly 8 mm – 80 mm, heavier plate to 100 mm by enquiry
- Width: 1500 mm – 3200 mm, wider by enquiry
- Length: 3000 mm – 12000 mm
Cut-to-size webs, flanges, base plates and gussets are available. Browse more sizes on structural steel plates.
Tolerances
Dimensional limits for Q390MC follow GB/T 709 unless the purchase order names EN 10029 or another table.
Typical thickness tolerance idea for Q390MC plate
| Nominal thickness (mm) | Usual minus (mm) | Usual plus (mm) |
|---|---|---|
| 8 – 15 | −0.3 | +0.8 |
| 15 – 25 | −0.4 | +0.9 |
| 25 – 40 | −0.5 | +1.1 |
| 40 – 60 | −0.6 | +1.3 |
| 60 – 80 | −0.7 | +1.5 |
| 80 – 100 | −0.8 | +1.6 |
Width on 1500–3200 mm plate is commonly held to about +20 / 0 mm or ±25 mm unless a tighter extra is named. Length on 3000–12000 mm plate is commonly held to about +50 / 0 mm. Flatness follows the agreed class. SHH STEEL will not assume a zero-minus extra on Q390MC unless the order says so.
Supplementary Requirements
Q390MC already defines 390 MPa yield, TMCP delivery and 0°C impact. Extra items still have to be written on the purchase order.
Book name. Write GB/T 1591 Q390MC. Do not write only Q390, and do not write Q390NC if the mill must stamp M. The family page is GB/T 1591.
Impact. Grade C is 0°C. Write a higher energy if the owner requires it. Do not expect a −20°C result unless the grade is changed.
Delivery condition. Write thermomechanical controlled process. Write GB/T 1591 Q390NC if normalized is required.
EN or US comparison. Write EN 10025-4 S420M or ASTM A572 Gr.55 only if dual mark is required and both tables are met.
Product analysis. Write it if the file needs the second chemistry column.
Through-thickness. Z15, Z25 or Z35 when the joint is loaded through the thickness.
NDE. UT to GB/T 2970 or the named class.
Identification. Heat number, Q390MC, thickness and mill logo.
Third-party witness. EN 10204 3.2 with SGS, TÜV, BV, ABS or the inspector named.
Applications
| Industry | Typical components |
|---|---|
| Buildings and workshops | Q390MC columns, beams and base plates |
| Bridges and towers | Q390MC webs and flanges from SHH STEEL |
| Construction machinery | Q390MC frames where the drawing names M and 0°C |
| General fabrication | Q390MC gussets and connection plates |
| Comparison vs EN 10025-4 | Q390MC next to EN 10025-4 S420M |
| Comparison vs ASTM A572 | Q390MC next to ASTM A572 Gr.55 |
| Lower yield option | GB/T 1591 Q355MD when 355 MPa is enough |
Q390MC is the plate for a 390 MPa TMCP file tested at 0°C. It is the wrong plate for a painted weathering facade that needs corten. It is the wrong plate for a 690 MPa QT boom under GB/T 16270. A colder 460 MPa normalized file is GB/T 1591 Q460NE.
Supply Capability
SHH STEEL sources Q390MC from first-line Chinese structural mills and ships it on worldwide terms. Partner mills include Wuyang (Wugang), Angang, Shougang, Hanye, Anyang Iron and Steel, Baosteel, Xinyu, Xingcheng and other qualified mills when the size requires it.
Mill test certificates are issued to EN 10204 3.1 as standard. EN 10204 3.2 is arranged when the order names a third-party hold point.
Usual rolling thickness: 8 mm, 10 mm, 12 mm, 16 mm, 20 mm, 25 mm, 30 mm, 40 mm, 50 mm, 60 mm, 80 mm. Heavier plate is confirmed before order.
Processing: CNC or flame cutting, bevel, flattening, shot blast, UT to the named class.
Trade terms: FOB Shanghai main, CIF destination available. Payment: TT, LC, or TT + LC.
Ocean time from Shanghai: US West 14–18 days; US Gulf 28–35 days; Rotterdam / Antwerp 28–35 days; Jebel Ali 18–25 days; Singapore 7–12 days; other ports quoted.
Third-party: SGS, TÜV, BV, ABS, CCS, GL, VL, DNV, RINA, NK, KR, or the inspector named.
Global Delivery and Markets
SHH STEEL is a global steel mill sourcing partner with mill partnerships in China. We supply GB, ASTM, ASME, EN, DIN and JIS steel to buyers in the United States, Europe, the Middle East, Southeast Asia, Africa and South America. Origin is mill-direct, China origin.
SHH STEEL has supplied steel plates to the USA, Mexico, Argentina, Peru, El Salvador, Spain, Netherlands, Germany, UAE, Saudi Arabia, South Africa, India, Thailand, Singapore, Vietnam, the Philippines, Japan and Korea.
Typical lead time: ex-stock 5–7 days when an M heat is in yard; standard TMCP about 25–40 days; 3.2 inspection about 35–45 days.
Why Choose SHH STEEL
SHH STEEL is a global steel mill sourcing partner and steel manufacturer and exporter, mill-direct, China origin. For Q390MC that means mill-direct structural price, not a multi-layer stockist mark-up. We buy from mills that can actually run the TMCP schedule, so the M is on the certificate and not only in the enquiry.
Delivery is short when the size is in rolling range: ex-stock 5–7 days, standard M heat about 25–40 days, 3.2 inspection about 35–45 days. Cutting, bevel and UT can run in the same window. FOB Shanghai is the main term. CIF to US West, US Gulf, Rotterdam, Jebel Ali and Singapore is quoted on the same file.
Experience on this grade is simple: print GB/T 1591 Q390MC, keep the TMCP route, and do not ship GB/T 1591 Q390NC as MC. We will not drop the M to save a cooling cycle, and we will not change C to B to save a cold test. If the drawing needs normalized plate, we will move the inquiry to Q390NC. If the drawing needs 420 MPa, we will move it to GB/T 1591 Q420ND or GB/T 1591 Q420NE.
FAQ
-
What is Q390MC steel plate?
- Q390MC in GB/T 1591-2018 is thermomechanical controlled process high-strength low-alloy plate with 390 MPa minimum yield on thin plate and Charpy impact at 0°C. SHH STEEL supplies this plate worldwide as a global steel mill sourcing partner.
-
Is Q390MC the same as Q390NC?
- No. Both yield at 390 MPa and both are tested at 0°C. Q390NC is normalized. Q390MC is TMCP.
-
Is Q390MC the same as Q390MB?
- No. Both are TMCP. Q390MB is tested at +20°C. Q390MC is tested at 0°C.
-
Is Q390MC the same as Q355MC?
- No. Both are TMCP and both are tested at 0°C. Q355MC is 355 MPa. Q390MC is 390 MPa.
-
What is the European equivalent of Q390MC?
- There is no S390 in EN 10025. EN 10025-4 S420M is the higher TMCP comparison. EN 10025-3 S420N is the normalized comparison. Dual mark only when both books are fully met.
-
What is the US equivalent of Q390MC?
- There is no official ASTM twin. ASTM A572 Grade 55 is 55 ksi / 380 MPa, slightly lower, and it does not carry an MC letter. SHH STEEL does not dual-mark ASTM A572 unless both books are met.
-
What thickness can SHH STEEL supply?
- Common supply is 8 mm to 80 mm. Plate to 100 mm is quoted by enquiry. Yield on plate over 16 mm is lower than the 390 MPa thin-plate number.
Conclusion
Q390MC steel plate to GB/T 1591 is 390 MPa TMCP structural plate with impact at 0°C. It is not normalized GB/T 1591 Q390NC. EN 10025 has no S390. EN 10025-4 S420M is a higher TMCP comparison. ASTM A572 Grade 55 is 380 MPa and is not a substitute. Whether the inquiry says Q390MC, GB/T 1591 Q390MC or Q390MC TMCP plate, SHH STEEL as a global steel mill sourcing partner supplies plate with Q390MC chemistry, heat and product analysis as ordered, GB/T 709 tolerances and EN 10204 3.1 or 3.2 certification.
SHH STEEL supplies Q390MC Steel Plate to the United States, Europe, the Middle East, Africa, Asia and the Americas for work that actually names the M condition. The grade family is listed on GB/T 1591.
Contact SHH STEEL for mill rolling, TMCP Q390MC, cutting, UT, 3.2 inspection or a worldwide quotation.
Q390MC, Q390MC steel plate, GB/T 1591 Q390MC, Q390MC TMCP, Q390MC supplier, SHH STEEL