GB/T 14976 06Cr19Ni9NbN Seamless Stainless Steel Pipe
What is GB/T 14976 06Cr19Ni9NbN Seamless Stainless Steel Pipe
Fluid-transport packages written to Chinese product standards look to GB/T 14976-2025 rather than inventing a mill grade from AISI shorthand alone. 06Cr19Ni9NbN is the Table 2/3 Chinese grade name for this austenitic chemistry (S30478). GB/T 14976 06Cr19Ni9NbN is not a marketing synonym for 304N — the Nb+N pair and 685 MPa Rm floor are why the mark exists.
Mill path for 06Cr19Ni9NbN: manufacture symbol W-C/W-H, Table 1 heat treatment, Table 2 cast chemistry, Table 3 tensile floors, hydrostatic or NDT per 7.3. SHH STEEL can make and supply the grade to that stack. Typical use: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
Body text may mention XM-21-class / Nb+N strengthened 304 (unified S30478) for cross-reference, but the H1 and order line stay on 06Cr19Ni9NbN. Silent alias swaps are how wrong carbon ceilings and wrong tensile tables enter the MTC. Keep this caution in view: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal.
Order the standard the drawing and regulatory file actually require. Inside this 14976 series, compare 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb, 06Cr19Ni10 before stretching surface finish or wall alone. Duty thread: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family. Document the medium, design temperature, and weld map beside the 06Cr19Ni9NbN line item so sister-grade swaps are engineering decisions rather than purchasing shortcuts. Application context for 06Cr19Ni9NbN stays high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
Inside this GB/T 14976 series, compare 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb, 06Cr19Ni10. Hub: GB/T 14976.
Chemical Composition of GB/T 14976 06Cr19Ni9NbN
Table 2 sets the melt limits for 06Cr19Ni9NbN. Highlight band: C ≤0.08, Si ≤1.00, Mn ≤2.00, P ≤0.035, S ≤0.030, Ni 7.50–10.50, Cr 18.00–20.00, N 0.15–0.30. Product analysis, when ordered, applies GB/T 222 stainless product tolerances on top of Table 2. Alias note: XM-21-class / Nb+N strengthened 304. Every ladle analysis for 06Cr19Ni9NbN is checked against those windows before the heat is released to piercing or drawing, and the same numbers reappear on the inspection document. Application context for 06Cr19Ni9NbN stays high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
The composition table below is the cast window SHH STEEL quotes against for 06Cr19Ni9NbN. Edition framing is GB/T 14976-2025. Use thread: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex. If a purchaser specification tightens phosphorus, sulphur, or residual elements beyond Table 2, SHH STEEL will confirm melt feasibility for 06Cr19Ni9NbN before the order is acknowledged. Weld-shop note tied to 06Cr19Ni9NbN: matching Nb-bearing or over-alloyed austenitic fillers; control heat input to protect stabilisation and nitrogen balance.
| Grade | C | Si | Mn | P | S | Ni | Cr | N | Nb |
|---|---|---|---|---|---|---|---|---|---|
| 06Cr19Ni9NbN | ≤0.08 | ≤1.00 | ≤2.00 | ≤0.035 | ≤0.030 | 7.50–10.50 | 18.00–20.00 | 0.15–0.30 | ≥0.15 |
Mechanical Properties of GB/T 14976 06Cr19Ni9NbN
Table 3 mechanical acceptance for 06Cr19Ni9NbN: Rm min 685 MPa, Rp0.2 min 345 MPa, elongation longitudinal min 35% / transverse min 30%. Delivery framing: solution annealed. Sampling follows chapter 8/10 rules for the batch of 06Cr19Ni9NbN. Tensile sampling follows the batch rules for the ordered test unit of 06Cr19Ni9NbN, and retests follow GB/T 2102 when a result sits under the Table 3 floor. Application context for 06Cr19Ni9NbN stays high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
| Grade | Rm min (MPa) | Rp0.2 min (MPa) | A long. min (%) | A trans. min (%) |
|---|---|---|---|---|
| 06Cr19Ni9NbN | 685 | 345 | 35 | 30 |
Ambient values from GB/T 14976-2025 Table 3 for 06Cr19Ni9NbN. Heat treatment (Table 1): 1010–1150 °C, water or rapid cool. Density 7.93 kg/dm³. Delivery: solution annealed.
Seamless Pipe Manufacture of GB/T 14976 06Cr19Ni9NbN
For 06Cr19Ni9NbN, the mill path is pierce/extrude/draw — never ERW or automatic-arc under GB/T 14976. Delivery is heat-treated and pickled unless overall ground/bored or bright protective-atmosphere treatment allows omitting pickle. Order W-C or W-H explicitly when the purchaser cares which route ships. Seamless W-C and W-H options remain available for 06Cr19Ni9NbN; the acknowledgement repeats the manufacture symbol so production cannot silently change route after the PO is firm. This paragraph is locked to 06Cr19Ni9NbN duty: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family.
After forming, 06Cr19Ni9NbN receives Table 1 treatment — 1010–1150 °C, water or rapid cool. Austenitic heats take solution annealing with water or other rapid cool per Table 1; hot-rolled austenitic pipe may count in-line rapid cool inside the Table 1 temperature band as meeting heat treatment (6.3.2) unless the purchaser forbids it. Use thread: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
Marking carries the grade 06Cr19Ni9NbN, manufacture cues, manufacturer ID, and GB/T 2102 items. Size hint: often cold-drawn W-C for high-strength mid-bore; confirm wall against the higher Table 3 floors. Weld thread for fabricator joints: matching Nb-bearing or over-alloyed austenitic fillers; control heat input to protect stabilisation and nitrogen balance. Hydrostatic pressure or NDT class for 06Cr19Ni9NbN is frozen with the size list so quality planners can book the correct benches before the pipe is cut to length. Corrosion framing beside 06Cr19Ni9NbN: corrosion still reads as Mo-free austenitic; strength, not chloride ranking, is why this mark exists.
Dimensions and Tolerances for GB/T 14976 06Cr19Ni9NbN
Dimensional order lines for 06Cr19Ni9NbN should state OD × wall (or ID × wall), length type, end finish, and PA or PC tolerance class. Use: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex. Tolerance class (PA/PC) follows the precision ordered for 06Cr19Ni9NbN, and out-of-table diameters are accepted only with a written dimensional agreement on the same acknowledgement. Application context for 06Cr19Ni9NbN stays high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
OD and wall tolerances differ for hot-finished W-H versus cold-finished W-C and for PA versus PC — quote the manufacture symbol with the size. Caution: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal. Fixed lengths and multiple cut lengths for 06Cr19Ni9NbN are protected at the ends so bevel geometry and ID cleanliness survive inland and ocean transit. Keep the 06Cr19Ni9NbN caution visible here: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal.
Equivalent Grades for GB/T 14976 06Cr19Ni9NbN
GB/T 14976 does not make XM-21-class / Nb+N strengthened 304 a drop-in certificate for 06Cr19Ni9NbN. Use the commercial name in dual-cert talk, then verify every Table limit that matters for this pipe. Sisters in the series are comparison pages, not interchangeable stock codes. Wall basis, tensile floors, and NDT clauses rarely map one-for-one even when the cast analysis looks familiar to a commercial alias (06Cr19Ni9NbN).
| System | Designation | Notes |
|---|---|---|
| GB/T 14976 | 06Cr19Ni9NbN | Governing pipe grade for this page |
| Commercial / UNS (body only) | XM-21-class / Nb+N strengthened 304 (unified S30478) | Useful in dual-cert talk; not a substitute on the PO/MTC |
| ASTM A312 related | 304 chemistry family | Related chemistry — different product standard; not interchangeable by default |
| EN / other | No one-to-one asserted | Starting point for comparison only against local product specs |
Inside this series compare 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb, 06Cr19Ni10 before swapping marks for medium or temperature. Confirm chemistry windows on the 06Cr19Ni9NbN MTC before dual-cert claims. Hub: GB/T 14976. Dual marking is a purchase-order option that still requires every limit that matters for 06Cr19Ni9NbN to be verified on the heat.
Heat Treatment and Delivery Condition for GB/T 14976 06Cr19Ni9NbN
Mill heat treatment for 06Cr19Ni9NbN: 1010–1150 °C, water or rapid cool. Bright annealing or overall machining may omit pickling when the surface is scale-free. Delivery label: solution annealed. Recorded furnace charts for 06Cr19Ni9NbN should support the Table 1 temperature claim on the certificate, including quench or cool method where the family requires rapid cooling. Size practice for 06Cr19Ni9NbN remains often cold-drawn W-C for high-strength mid-bore; confirm wall against the higher Table 3 floors.
Certificate wording for 06Cr19Ni9NbN should show the heat-treatment condition actually performed, not a generic “annealed” stamp that hides temperature. Use: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex. Field heat treatment of 06Cr19Ni9NbN after hot bending must chase the same family practice, or the corrosion file should formally accept the as-bent condition. Corrosion framing beside 06Cr19Ni9NbN: corrosion still reads as Mo-free austenitic; strength, not chloride ranking, is why this mark exists.
Corrosion Resistance of GB/T 14976 06Cr19Ni9NbN
corrosion still reads as Mo-free austenitic; strength, not chloride ranking, is why this mark exists Special Annex A cryogenic or Annex B oxygen extras are not a blanket corrosion warranty. Family filing: austenitic. Clause 7.5 requires intergranular corrosion testing (GB/T 4334 method E) for austenitic 06Cr19Ni9NbN unless the mark is one of the four carbon-floor exemptions.
Do not market invented PREN digits. Bring medium chemistry and SHH STEEL will map 06Cr19Ni9NbN honestly against 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb, 06Cr19Ni10. Role: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family. If operating chlorides, temperature, or crevice geometry change after award, reopen the alloy choice for 06Cr19Ni9NbN rather than relying on wall thickness alone. Weld-shop note tied to 06Cr19Ni9NbN: matching Nb-bearing or over-alloyed austenitic fillers; control heat input to protect stabilisation and nitrogen balance.
Applications of GB/T 14976 06Cr19Ni9NbN Seamless Pipe
Typical BOM language pairs GB/T 14976 06Cr19Ni9NbN with OD × wall, W-C or W-H, PA/PC, and heat-treatment condition. Primary sketch: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex. Spool fabricators should copy 06Cr19Ni9NbN onto cut lists and WPS bases so warehouse substitutions cannot quietly introduce a different carbon or molybdenum window. Application context for 06Cr19Ni9NbN stays high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
Spell 06Cr19Ni9NbN on isometrics, spool sheets and valve specs alike. Sister options when the medium hardens: 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb, 06Cr19Ni10. Commissioning teams benefit when the as-built dossier repeats 06Cr19Ni9NbN beside heat numbers, linking isometric revisions to the same mill certificates. Corrosion framing beside 06Cr19Ni9NbN: corrosion still reads as Mo-free austenitic; strength, not chloride ranking, is why this mark exists.
Weldability of GB/T 14976 06Cr19Ni9NbN
Weldability of 06Cr19Ni9NbN follows austenitic practice. Filler/shop note: matching Nb-bearing or over-alloyed austenitic fillers; control heat input to protect stabilisation and nitrogen balance. Caution: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal. Procedure qualification for 06Cr19Ni9NbN should use the same product form and wall class as production, including the seamless finish that will ship. Application context for 06Cr19Ni9NbN stays high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
For corrosive as-welded duty on 06Cr19Ni9NbN, confirm low-carbon, stabilisation, or anneal practice as applicable. Shop note: matching Nb-bearing or over-alloyed austenitic fillers; control heat input to protect stabilisation and nitrogen balance. Consumable lot control and shielding-gas notes for 06Cr19Ni9NbN stay with the WPS package so site crews cannot improvise fillers that under-alloy the joint. Corrosion framing beside 06Cr19Ni9NbN: corrosion still reads as Mo-free austenitic; strength, not chloride ranking, is why this mark exists.
Surface Finishes for GB/T 14976 06Cr19Ni9NbN
06Cr19Ni9NbN under GB/T 14976 typically ships solution annealed and pickled so scale and heat tint are removed before installation. Bright anneal covers appearance orders; special roughness is by agreement. Role: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family. Free-iron control continues through storage and shipment, because late carbon-steel contact can stain an otherwise clean pickle (06Cr19Ni9NbN).
| Finish | Typical supply | Order note |
|---|---|---|
| Solution annealed and pickled | Standard pipe mill finish after solution anneal | Matte, scale-free after pickling |
| Bright annealed | When scale-free OD/ID appearance is ordered | State OD, ID, or both |
| Ground / polished | By agreement for roughness callouts | Name Ra/grit and which surface; no invented default grit |
| Passivated | When end-user spec requires (e.g. A967 analogue) | Not a substitute for correct heat treatment |
SHH STEEL sequences pickle, optional passivation, and any agreed polish for 06Cr19Ni9NbN after the heat-treatment evidence is on the certificate. Free-iron control and packing discipline matter as much as Ra numbers for long pipe life in the field. Final visual release still rejects grinding burns, embedded free iron, and unrepaired weld undercut before bundles are closed (06Cr19Ni9NbN).
Inspection and Testing for GB/T 14976 06Cr19Ni9NbN
SHH STEEL reports the tests actually performed for 06Cr19Ni9NbN — no surrogate NDT lines. Hydrostatic vs eddy-current/ultrasonic choice belongs on the PO when replacement is allowed. Caution: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal. Sampling plans for 06Cr19Ni9NbN keep heat identity unbroken from melt through bundle tags, including any third-party hold points written into the purchase order. This paragraph is locked to 06Cr19Ni9NbN duty: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family.
NDT acceptance defaults to GB/T 5777 U3 or GB/T 7735 E4H/E4 when UT/ET replace hydro; Annex A/B may tighten to U2.5. Size context: often cold-drawn W-C for high-strength mid-bore; confirm wall against the higher Table 3 floors. Non-conforming 06Cr19Ni9NbN lengths are segregated and retested or rejected under GB/T 2102 rather than reworked into unmarked stock. Size practice for 06Cr19Ni9NbN remains often cold-drawn W-C for high-strength mid-bore; confirm wall against the higher Table 3 floors.
Packaging and Shipping for GB/T 14976 06Cr19Ni9NbN
Export packing for GB/T 14976 06Cr19Ni9NbN is built around rust prevention and transit abrasion control. Bundle tickets repeat the grade symbol and heat number. Duty: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family. Bundle tickets for 06Cr19Ni9NbN repeat grade, heat, size, and quantity so receiving inspectors can match crates to the packing list without opening every wrap. This paragraph is locked to 06Cr19Ni9NbN duty: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family.
Marking paint and ink stickers stay chloride-lean. Heat numbers on tags match the MTC for 06Cr19Ni9NbN. Desiccant and wrap choices for 06Cr19Ni9NbN follow the voyage length and storage climate stated on the shipping order, not a one-size export habit. Keep the 06Cr19Ni9NbN caution visible here: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal.
Photographic packing records are available on request for project QA files on 06Cr19Ni9NbN. Claims handling for 06Cr19Ni9NbN starts with tagged photos against the packing list so heat identity remains usable if replacement lengths are required. Application context for 06Cr19Ni9NbN stays high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex.
Why Choose SHH STEEL
Buyers choose SHH STEEL for 06Cr19Ni9NbN because the paperwork matches the stencil: Table 2 chemistry, Table 3 tensile, Table 1 heat treatment, and honest seamless marking. Application fit: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex. SHH STEEL can produce and supply 06Cr19Ni9NbN against the OD × wall, seamless route, and test scope on your RFQ without swapping in an unstated sister grade.
SHH STEEL will not invent PREN posters or warehouse tonnages. Bring OD × wall, medium notes, and test scope — we will quote 06Cr19Ni9NbN cleanly. Ask for a written acknowledgement that names 06Cr19Ni9NbN, W-C or W-H, and the Table 1 heat-treatment condition before melt. SHH STEEL can make 06Cr19Ni9NbN to that written scope.
Supply Capability
Supply capability for 06Cr19Ni9NbN covers seamless manufacture symbols, Table 1 heat treatment, and Table 3 mechanical acceptance. SHH STEEL can make the sizes on your list when the mill slot fits. Role: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family. SHH STEEL can produce and supply cut lengths, bevels, and ordered annex tests for 06Cr19Ni9NbN when the mill schedule allows.
| Item | Capability |
|---|---|
| Standard | GB/T 14976-2025 seamless stainless steel pipes for fluid transport |
| Grade | 06Cr19Ni9NbN (S30478) |
| Product form | Seamless pipe only — cold-rolled/drawn (W-C) or hot-rolled/extruded/forged/expanded (W-H) |
| Delivery condition | solution annealed |
| Documents | Mill test certificate (GB/T 2102 / EN 10204 3.1 style as ordered) |
| Typical size practice | OD × wall per GB/T 17395; PA ordinary or PC higher precision; usual length 4000–12000 mm |
| Wall / ordering | Nominal OD×wall, OD×min wall, or ID×wall by agreement |
Stock / Available sizes
Stock / Available sizes for 06Cr19Ni9NbN: common OD×wall combinations as the project uses. Seamless W-C versus W-H availability varies by diameter — confirm route with the RFQ. Hint: often cold-drawn W-C for high-strength mid-bore; confirm wall against the higher Table 3 floors. SHH STEEL can supply alternate walls and precision classes for 06Cr19Ni9NbN once the design pressure and corrosion allowance are clear.
Mill certificates, packing photos, and third-party witness can be bundled into the 06Cr19Ni9NbN supply scope when the PO says so. Use: high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex. SHH STEEL can produce trial lengths of 06Cr19Ni9NbN for procedure qualification before the bulk release when the project calendar needs it.
FAQ
-
What is GB/T 14976 06Cr19Ni9NbN seamless stainless steel pipe used for?
- GB/T 14976 06Cr19Ni9NbN is seamless stainless pipe for fluid transport — high-pressure fluid headers, compact skid piping, and Chinese designs that need Rm near 685 MPa without jumping to duplex. Role summary: Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family. It is a Chinese product standard grade (S30478), not an automatic ASTM A312 certificate.
-
Is GB/T 14976 06Cr19Ni9NbN seamless only, or does it cover welded pipe?
- Seamless only. Clause 6.2 limits manufacture to cold-rolled/drawn (W-C) or hot-rolled/extruded/forged/expanded (W-H) seamless routes. SHH STEEL can produce and supply either seamless route for 06Cr19Ni9NbN when the mill can meet the ordered size and tests. Welded pipe belongs under other standards, not 14976.
-
What heat treatment applies to 06Cr19Ni9NbN?
- 06Cr19Ni9NbN is delivered solution annealed under GB/T 14976. Table 1 reference: 1010–1150 °C, water or rapid cool. Other schedules need written agreement. Certificate wording should match the treatment actually performed. Keep the purchase order locked to GB/T 14976 and 06Cr19Ni9NbN so cast limits, heat treatment, and seamless W-C/W-H marking stay unambiguous on the mill certificate.
-
How does 06Cr19Ni9NbN compare with sister grades 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb?
- 06Cr19Ni9NbN is filed as austenitic. Typical sisters on the same RFQ are 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb. Design caution: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal Pick the sister when the medium or strength floor outgrows this grade rather than stretching wall alone.
-
What tests appear on the mill certificate for 06Cr19Ni9NbN?
- Expect cast analysis (Table 2), room-temperature tensile results (Table 3), dimensions, hydrostatic test (or replacing UT/ET), appearance, and every special annex or IGC test actually performed. SHH STEEL does not print surrogate inspection lines. Documents follow GB/T 2102 or EN 10204 3.1 style when specified.
-
Is XM-21-class / Nb+N strengthened 304 the same as ordering 06Cr19Ni9NbN?
- No. XM-21-class / Nb+N strengthened 304 is a commercial / UNS cross-walk for body text (unified S30478). The purchase order should lock GB/T 14976 and 06Cr19Ni9NbN so cast limits, heat treatment, and seamless route are unambiguous. Silent alias substitution is a common root cause of wrong MTCs.
-
What size range can SHH STEEL quote for GB/T 14976 06Cr19Ni9NbN?
- SHH STEEL can produce and supply enquiry-oriented OD × wall bands for 06Cr19Ni9NbN within GB/T 17395 practice, with PA or PC precision and measured or min-wall options by agreement. Size context: often cold-drawn W-C for high-strength mid-bore; confirm wall against the higher Table 3 floors. Stock / Available sizes on this page is an RFQ map, not a frozen tonnage catalogue.
-
How should 06Cr19Ni9NbN be welded on site?
- Shop guidance: matching Nb-bearing or over-alloyed austenitic fillers; control heat input to protect stabilisation and nitrogen balance. Mill heat treatment of seamless pipe does not replace a qualified WPS on fabricator joints. For corrosive as-welded duty, confirm low-carbon, stabilisation, or anneal practice as applicable. Caution: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal
-
When should I choose a higher-Mo or superaustenitic grade instead of 06Cr19Ni9NbN?
- Move when chloride pitting, crevice attack, or reducing-acid risk exceeds what austenitic practice can defend for the temperature and stress state. Caution for this mark: Nb ≥0.15 and N 0.15–0.30 are intentional — do not substitute plain 06Cr19Ni10N; weld procedure must respect Nb-bearing base metal Sister pointers: 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb. SHH STEEL will not invent PREN marketing digits — bring the medium data.
-
Can SHH STEEL dual-certify GB/T 14976 06Cr19Ni9NbN with ASTM A312?
- Dual documentation is possible only when chemistry and tests satisfy each standard on its own terms. An MTC that only cites GB/T 14976 06Cr19Ni9NbN does not clear ASTM acceptance by default. State both standards, sizes, and test scopes before melt. Keep the purchase order locked to GB/T 14976 and 06Cr19Ni9NbN so cast limits, heat treatment, and seamless W-C/W-H marking stay unambiguous on the mill certificate.
-
What surface finishes are available for 06Cr19Ni9NbN?
- Pickled after heat treatment is the usual fluid-transport supply. Bright anneal, grind, or polish finishes are by agreement and must state OD/ID scope. SHH STEEL can produce and supply the ordered finish for 06Cr19Ni9NbN when the mill route supports it. Carbon-steel strapping never contacts the stainless OD.
Conclusion
GB/T 14976 06Cr19Ni9NbN is seamless stainless steel pipe for fluid transport — Nb+N strengthened austenitic seamless pipe for high-strength fluid service still inside the 18-8 chromium-nickel family. SHH STEEL can produce and supply it in cold-finished or hot-finished seamless routes with the heat treatment, tests, and finishes named on your enquiry, documented on mill certificates. Sister grades often discussed alongside this mark include 06Cr19Ni10N, 022Cr19Ni10N, 06Cr18Ni11Nb. Related ASTM pages share chemistry families but not Chinese acceptance text. Email admin@steelspecs.com with OD × wall, W-C or W-H preference, and medium notes to start the quote.