EN 10217-7 1.4404 Welded Stainless Steel Tube

EN 10217-7 1.4404 / X2CrNiMo17-12-2 welded stainless pressure tube (316L), austenitic, cast analysis per EN table, ambient Rp0.2 min 190 MPa, Rm 490–690, solution annealed 1020–1120 °C. SHH STEEL can produce and supply with EN 10204 3.1 MTCs, TC1/TC2 testing.
Grade
1.4404 / X2CrNiMo17-12-2 (316L — body alias)
Standard
EN 10217-7
Product form
Welded tube for pressure purposes (longitudinal arc/laser), solution annealed as required by delivery condition
Size
~6–219 mm OD × 0.5–12.7 mm wall within family characterisation; other sizes by agreement
Share:
Overview
Chemical Composition
Mechanical Properties
Welded Tube Manufacture
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is EN 10217-7 1.4404 Welded Stainless Steel Tube

When an enquiry still reads “316L welded pressure tube” without a European product standard, the PED paperwork is incomplete. EN 10217-7:2021 closes that gap for circular welded austenitic and duplex stainless tubes; within that list, 1.4404 / X2CrNiMo17-12-2 is the austenitic entry that matches this chemistry. SHH STEEL treats the steel number, not the shop alias, as the acceptance key on cast analysis, longitudinal arc or laser seam route, solution annealing where the delivery symbol requires it, and the TC1/TC2 inspection regime. Duty focus: low-carbon Mo-bearing austenitic for welded pressure tube in chloride-bearing and chemical PED service where 316L chemistry is the buyer’s default.

SHH STEEL can produce and supply EN 10217-7 1.4404 welded stainless steel tube — longitudinally arc- or laser-welded from strip or plate on the standard’s manufacturing routes, solution annealed where the ordered delivery condition requires it, with EN 10204 3.1 inspection documents (3.2 under Option 21) reporting cast chemistry and ambient mechanical results against the ordered edition. Typical enquiry sizes cover widest commercial welded OD×wall band in the Mo austenitic family for EN 10217-7. Browse the series hub at EN 10217-7.

Most “316L welded pressure tube” European enquiries resolve to EN 10217-7 1.4404 once the purchaser stops accepting ASTM A312/A269 text as PED acceptance. Typical welded pressure duties include coastal utilities, brine-adjacent process lines, pharmaceutical and food lines with chloride sanitiser exposure, and general chemical PED piping. Design caution: 316L-family still has chloride SCC limits under tensile stress and temperature — duplex 1.4462 is often the next step when SCC governs Commercially the grade is often called 316L; keep that name on the enquiry note and in the body, never as a substitute for steel number 1.4404 / X2CrNiMo17-12-2 on the MTC. Sister numbers on this hub include EN 10217-7 1.4401, EN 10217-7 1.4432, EN 10217-7 1.4435, EN 10217-7 1.4462.4401, 1.4432, 1.4435, 1.4462.

Welded-only scope matters on every 1.4404 order. Seamless sisters are a different standard (EN 10216-5). Sizes prefer EN ISO 1127. Table 1 manufacture is longitudinal automatic arc or laser from strip/plate; do not specify spiral and expect automatic Part 7 acceptance without a written agreement outside the listed routes. Live seamless sister: EN 10216-5 1.4404. Related live ASTM/ASME anchors: A269 TP316L, A213 TP316L, SA213 TP316L, A312 TP316L, SA312 TP316L.

Chemical Composition of EN 10217-7 1.4404

Ladle analysis controls 1.4404. The austenitic table entry for X2CrNiMo17-12-2 is what the cast must satisfy; product analysis remains Option 6. SHH STEEL’s EN 10204 paperwork shows real cast results — catalogue “typical” chemistries are not substituted for EN acceptance on 316L-class welded pressure tube.

Below is the BSSA-published EN 10217-7 cast window for X2CrNiMo17-12-2 (steel number 1.4404), aligned to the 2021 list. Maxima apply unless a min–max range appears. Edition confirmation beats brochure reprint.

Element 1.4404 cast analysis (mass %)
Carbon (C) ≤0.030
Silicon (Si) ≤1.00
Manganese (Mn) ≤2.00
Phosphorus (P) ≤0.045
Sulfur (S) ≤0.015
Nitrogen (N) ≤0.10
Chromium (Cr) 16.5–18.5
Nickel (Ni) 10.0–13.0
Molybdenum (Mo) 2.0–2.5

Chemistry source for steel number 1.4404: BSSA EN 10217-7 chemical article plus public standard cross-check. Do not treat unlisted elements as free additions on X2CrNiMo17-12-2 without purchaser agreement (finishing additions excepted under controlled scrap practice).

Mechanical Properties of EN 10217-7 1.4404

For X2CrNiMo17-12-2 ordered as EN 10217-7 1.4404, room-temperature mechanical acceptance follows the austenitic ambient table in the solution-annealed (+AT) condition within about 60 mm wall unless Options extend the band. Expect Rp0.2 and Rp1.0 minima plus Rm and elongation. Cryogenic Charpy characterisation exists; tested joules require the relevant Options.

Primary ambient source for 1.4404: BSSA mechanical properties for stainless steels to BS EN 10217-7. Heat-treatment bands for X2CrNiMo17-12-2 are public EN stainless figures with an UNCERTAIN flag against paid EN 10217-7:2021 footnotes. Sister-standard tensile values are not silently copied onto this Part 7 document.

Property 1.4404 ambient (solution annealed +AT)
Rp0.2 min (MPa) 190
Rp1.0 min (MPa) 225
Rm (MPa) 490–690
A min % long / trans 40 / 30
IGC resistance (delivery) Yes (method A)
Solution annealing (public EN band) 1020–1120 °C — UNCERTAIN vs paid EN 10217-7:2021 footnote if diverges
Cooling water or air
Charpy sub-zero (transverse min J) 60 at -196 °C (Option to verify)

Ambient mechanical citation for steel number 1.4404: BSSA EN 10217-7 article; annealing bands public EN cross-check (UNCERTAIN vs paid 2021 footnotes). Order impact Options when tested toughness for X2CrNiMo17-12-2 must be certified.

Welded Tube Manufacture for EN 10217-7 1.4404

For austenitic grade 1.4404, Part 7 manufacture starts with strip or plate of X2CrNiMo17-12-2 chemistry, forms a circular section, and closes it with a longitudinal automatic arc or laser weld per Table 1. Filler may or may not be used depending on route and wall. Outside grinding or bead working before heat treatment appear where the ordered path requires them. Commodity sizes usually run on continuous strip lines; heavier walls move to plate forming. Spiral weld is not invented here as a standard Part 7 route. Seamless product is a different standard — EN 10216-5.

Molybdenum-bearing austenitic 1.4404 (X2CrNiMo17-12-2) uses the same longitudinal arc/laser Table 1 routes, typically without filler or with matching Mo-bearing filler by wall and procedure. Options 3 and 4 cover inside remelt or bead working for smoothed ID. Delivery symbols W0–W2R, WCA/WCR, WG/WP follow Table 2; Option 5 locks the choice. SHH STEEL can produce and supply 1.4404 as W1A/W2A descaled or WCA/WCR cold-finished in the common pressure-tube band, and as WG/WP when roughness scope is agreed. 316L-class fillers; control heat input and ferrite; mill anneal of the tube is not a fabricator PWHT substitute

Put TC1 or TC2 on the 1.4404 enquiry before slots are booked. That choice drives tensile sampling and weld-seam NDT weight; leak-tightness still hits every tube (Option 15 to choose the method). Mill documents from SHH STEEL list the manufacturing route and delivery symbol applied to X2CrNiMo17-12-2.

Dimensions and Tolerances for EN 10217-7 1.4404

Specify D and T when buying EN 10217-7 1.4404 (X2CrNiMo17-12-2). EN ISO 1127 preferred sizes are the usual starting list; mass uses stainless density tables. Diameter/wall classes follow Part 7 with EN ISO 1127, including Option 20 D4. Out-of-roundness and eccentricity are absorbed inside those tolerances; weld-edge radial mismatch is separately limited.

Cut-to-length (Option 19) and bevelled ends (Option 18, wall ≥ 3.2 mm) are everyday extras on X2CrNiMo17-12-2 welded tube. Tighter OD conversations usually move toward WCA/WCR. SHH STEEL matches the ordered D × T, tolerance class, and delivery symbol before committing 1.4404 weld capacity.

Route / condition Typical use Notes
W1 / W1A / W1R Hot-rolled starting flat product Descaled or bright-annealed per symbol
W2 / W2A / W2R Cold-rolled starting flat product Smoother OD than W1 family except at weld
WCA / WCR Cold finished ≥20% after weld Recrystallized weld metal; OD often ≤168.3 mm
WG / WP Ground / polished Agree ID/OD scope and grit at enquiry

For X2CrNiMo17-12-2 welded tube, SHH STEEL verifies OD, wall, and the selected tolerance class on EN 10217-7 1.4404 before marking. Straightness and end-finish rules in the dimensional clauses still apply — they are not waived by a tight delivery promise. SHH STEEL confirms OD × wall and the selected EN ISO 1127 / Part 7 tolerance class for 1.4404 / X2CrNiMo17-12-2 on the inspection document rather than assuming mid-tolerance catalogue values.

Equivalent Grades for EN 10217-7 1.4404

Designation discipline: EN 10217-7 writes 1.4404 / X2CrNiMo17-12-2; shops say 316L. Related ASTM/ASME product pages are cross-references only — wall basis, tensile tables, and inspection differ. EN 10216-5 seamless pages are chemistry cousins with a different manufacture and acceptance route.

Bill-of-materials writers sometimes list 316L next to EN and ASTM numbers interchangeably. For this product, steel number 1.4404 with name X2CrNiMo17-12-2 under EN 10217-7 is the welded acceptance path; confirm any dual mark against both mechanical tables before release to fabrication.

Reference Designation Note
EN 10217-7 1.4404 / X2CrNiMo17-12-2 This product standard (welded pressure tube)
EN steel name X2CrNiMo17-12-2 EN 10027-1 designation used in body and marking
Commercial alias (body only) 316L Not a substitute for the steel number on the MTC
EN 10216-5 (seamless sister) 1.4404 Related live page — different product form (seamless)
A269 TP316L A269 TP316L Related live page — different product standard
A213 TP316L A213 TP316L Related live page — different product standard
SA213 TP316L SA213 TP316L Related live page — different product standard
A312 TP316L A312 TP316L Related live page — different product standard
SA312 TP316L SA312 TP316L Related live page — different product standard

Inside this welded series, compare EN 10217-7 1.4401, EN 10217-7 1.4432, EN 10217-7 1.4435, EN 10217-7 1.4462. Hub: EN 10217-7. Seamless sister: EN 10216-5 1.4404. Live cross-standard anchors: A269 TP316L, A213 TP316L, SA213 TP316L, A312 TP316L, SA312 TP316L.

Heat Treatment and Delivery Condition for EN 10217-7 1.4404

For X2CrNiMo17-12-2 ordered as 1.4404, pick a Table 2 symbol that encodes the required heat treatment and surface. Solution annealing (+AT) underpins the ambient mechanical table: bring the tube into the solution-temperature window and cool quickly enough to satisfy strength and corrosion notes. For X2CrNiMo17-12-2 under steel number 1.4404, keep Option 5 in mind when the delivery-condition symbol must be contractual, and reconcile the certificate wording with the solution-annealing practice actually used on the welded tube before releasing the PED file.

Solution band used on this page for 1.4404: 1020–1120 °C, cool by water or air (public EN stainless cross-check; UNCERTAIN vs paid EN 10217-7:2021 footnotes). Lock the delivery-condition symbol with Option 5 when pickle versus bright anneal versus WG/WP must be contractual for X2CrNiMo17-12-2.

Item 1.4404
Solution annealing band (public) 1020–1120 °C (UNCERTAIN vs paid Part 7 footnote)
Cooling water or air
Delivery condition symbols W0 / W1 / W1A / W1R / W2 / W2A / W2R / WCA / WCR / WG / WP (Option 5 to specify)
Inspection document EN 10204 3.1 default; 3.2 under Option 21

Heat-treatment honesty is part of the X2CrNiMo17-12-2 supply package: SHH STEEL documents the delivery-condition symbol actually run on EN 10217-7 1.4404, including whether the longitudinal weld was recrystallized on cold-finished routes, rather than implying a generic “annealed” stamp without Table 2 language. For X2CrNiMo17-12-2 under steel number 1.4404, keep Option 5 in mind when the delivery-condition symbol must be contractual, and reconcile the certificate wording with the solution-annealing practice actually used on the welded tube before releasing the PED file.

Corrosion Resistance of EN 10217-7 1.4404

Choose 1.4404 (X2CrNiMo17-12-2) when welded PED tubing must carry this corrosion story: ~2–2.5% Mo improves pitting and crevice resistance versus Mo-free 18-8; low carbon supports as-welded IGC behaviour. Delivery-condition IGC resistance is characterised to EN ISO 3651-2 methods in the Part 7 tables, but a tested IGC result still requires Option 13 on the order.

Long-service IGC temperature guidance in the standard is about sensitisation risk, not allowable stress. If the chloride or acid duty exceeds what this chemistry supports, step to EN 10217-7 1.4401, EN 10217-7 1.4432, EN 10217-7 1.4435, EN 10217-7 1.4462. SHH STEEL will not invent PREN or CPT acceptance floors for EN 10217-7 1.4404 / X2CrNiMo17-12-2.

Applications of EN 10217-7 1.4404 Tube

Applications for steel number 1.4404 / X2CrNiMo17-12-2 cluster around welded PED service that tolerates a mill seam: coastal utilities, brine-adjacent process lines, pharmaceutical and food lines with chloride sanitiser exposure, and general chemical PED piping. Delivery condition and test category on the order decide how that tube is finished and inspected before it reaches the spool.

Skip 1.4404 when the specification locks seamless product (EN 10216-5 — see EN 10216-5 1.4404), when ASTM A269/A312 text is the only acceptance language, or when corrosion/strength clearly points at another family. SHH STEEL can produce and supply X2CrNiMo17-12-2 welded tube in the enquiry band and will redirect to a sister or live ASTM/ASME page when that is wiser. Related live pages: A269 TP316L, A213 TP316L, SA213 TP316L, A312 TP316L, SA312 TP316L.

Weldability of EN 10217-7 1.4404

Mill welding of EN 10217-7 1.4404 is the longitudinal arc/laser seam on the ordered Table 1 route; field or shop welding is a separate PED joint design. Filler and procedure choices track the austenitic chemistry of X2CrNiMo17-12-2. Practical note: 316L-class fillers; control heat input and ferrite; mill anneal of the tube is not a fabricator PWHT substitute

PED joint design — including whether X2CrNiMo17-12-2 can remain as-welded in corrosive service — is outside mill scope. SHH STEEL’s deliverable for 1.4404 is compliant welded tube with documented chemistry, route, delivery condition, mechanical results, and leak/NDT statements.

Surface Finishes for EN 10217-7 1.4404

For X2CrNiMo17-12-2 welded under EN 10217-7 1.4404, finish language equals Table 2 language: descaled for utility, bright-annealed for cleaner OD, ground or polished when roughness is contractual. Agree WP/WG at enquiry with inspectable criteria. Transit contact with carbon steel is forbidden because free-iron rust blooms on 316L OD fail goods-in visual checks and contaminate stainless systems downstream of the weld seam.

Special ID finishes are order lines. When measurement is possible, SHH STEEL can produce and supply pickled, bright-annealed, and polished 1.4404; we will not invent an Ra number for 316L or imply electropolish that was never run on X2CrNiMo17-12-2. Exterior polish without an agreed grit is equally unacceptable as certificate language.

When 316L welded tube must look like instrumentation stock, bright anneal or polish belongs on the order with 1.4404. Descaled W1A/W2A remains correct for many lagged utility runs. SHH STEEL can produce and supply only the finish path X2CrNiMo17-12-2 can actually certify under EN 10217-7 on the promised date.

Inspection and Testing for EN 10217-7 1.4404

For EN 10217-7 1.4404 / X2CrNiMo17-12-2, expect cast chemistry per heat, ambient tensile at TC1/TC2 frequency, technological tests from the standard’s table, and 100% leak-tightness (hydrostatic or eddy current). Dimensional, visual, and material-identification checks close the baseline regime. Keep TC1/TC2, Option 13 IGC, and any impact Options visible on the 1.4404 purchase order so X2CrNiMo17-12-2 inspection planning matches the PED file before weld slots are locked.

Heavier weld-seam NDT is the TC2 differentiator on 1.4404. Laminar/edge NDT Options, IGC Option 13, and Charpy Options are purchaser choices. SHH STEEL’s EN 10204 3.1 file records what was melted, how X2CrNiMo17-12-2 was heat-treated, what tensile was achieved, and which leak/NDT path ran — without skipping required tests for speed.

If the end user specification layers project NDT on top of EN 10217-7, write those extras beside TC1/TC2 on the 1.4404 enquiry. SHH STEEL will map what Part 7 already covers for X2CrNiMo17-12-2 and what must be added by agreement, instead of discovering gaps after the tubes are bundled.

Packaging and Shipping for EN 10217-7 1.4404

SHH STEEL ships EN 10217-7 1.4404 in end-protected, size-sorted bundles or wooden crates with waterproof wrapping for sea freight. Bright-annealed and polished OD (W1R/W2R, WCR, WP) take sleeve or paper wrap against transit galling; descaled W1A/W2A utility tube still needs clean supports under the longitudinal seam. Because X2CrNiMo17-12-2 is stainless, packing deliberately keeps carbon-steel strapping and rusty fixtures off the tube surface — free-iron transfer is a common transit complaint on 316L and is prevented at the dock, not debated later.

Traceability marking on X2CrNiMo17-12-2 welded tube carries EN 10217-7, steel number 1.4404, size, cast, test category, and inspection/correlation marks. Delivery symbols are added when ordered or when clarity helps receiving. SHH STEEL aligns stencil language with the PO before dispatch. SHH STEEL treats packing and marking for EN 10217-7 1.4404 / X2CrNiMo17-12-2 as part of product conformity, not as a warehouse afterthought, so the PED receiving inspection sees protected ends, clean contact materials, and stencil text that matches the certificate.

Heat-to-bundle correlation on export documents saves receiving time for 316L welded tube. Cut-to-length and bevelled lots are packed apart with caps fitted. SHH STEEL applies the agreed packing note on every 1.4404 shipment. SHH STEEL treats packing and marking for EN 10217-7 1.4404 / X2CrNiMo17-12-2 as part of product conformity, not as a warehouse afterthought, so the PED receiving inspection sees protected ends, clean contact materials, and stencil text that matches the certificate.

Why Choose SHH STEEL

SHH STEEL can produce and make EN 10217-7 1.4404 welded pressure tube for buyers who need documented X2CrNiMo17-12-2 chemistry, delivery-condition heat treatment, and leak-tightness — not a shop-floor 316L stamp. We refuse to blur this page into EN 10216-5 seamless acceptance or to decorate MTCs with foreign tensile floors.

When 316L is the wrong tool, SHH STEEL steers toward EN 10217-7 LINKPLACE1.4401, EN 10217-7 LINKPLACE1.4432, EN 10217-7 LINKPLACE1.4435, EN 10217-7 LINKPLACE1.4462. Keep this caution in view: 316L-family still has chloride SCC limits under tensile stress and temperature — duplex LINKPLACE1.4462 is often the next step when SCC governs A mis-selected steel number helps no PED dossier. Live ASTM/ASME anchors: A269 TP316L, A213 TP316L, SA213 TP316L, A312 TP316L, SA312 TP316L.

Supply Capability

SHH STEEL can produce and supply welded EN 10217-7 1.4404 when your enquiry states standard edition, test category, delivery condition, and options. Capability and Stock / Available sizes tables below support first sizing for this 316L pressure grade. Widest commercial welded od×wall band in the mo austenitic family for en 10217-7.

Item SHH STEEL capability for 1.4404
Standard EN 10217-7
Grade 1.4404 / X2CrNiMo17-12-2
Product form Welded tube for pressure purposes (longitudinal arc/laser), solution annealed as required by delivery condition
Delivery condition W0 / W1 / W1A / W1R / W2 / W2A / W2R / WCA / WCR / WG / WP (Option 5 to lock)
Typical size band ~6–219 mm OD × 0.5–12.7 mm wall within family characterisation; other sizes by agreement
Testing TC1 or TC2; leak-tightness each tube; weld-seam NDT per category / options
Documents EN 10204 3.1 (3.2 Option 21); third-party inspection on request

Stock / Available sizes

Treat the size map as availability language for 316L welded pressure tube, not a tonnage inventory. 1.4404 depends on X2CrNiMo17-12-2 flat-product supply and weld finishing. Confirm against your OD × wall and TC1/TC2 list.

OD (mm) Typical walls (mm) Notes
12 / 14 / 16 / 19 / 21.3 / 25 1.0 / 1.5 / 2.0 / 2.5 Instrument / hygienic; often WCA/WCR or W2R
26.9 / 33.7 / 38 / 42.4 / 48.3 1.5 / 2.0 / 2.5 / 3.0 / 4.0 Process and utility welded pressure tube
60.3 / 76.1 / 88.9 / 114.3 2.0 / 3.0 / 4.0 / 5.0 / 6.0 Utility and process; lock W1A/W2A vs WCA
141.3 / 168.3 / 219.1 3.0 / 4.0 / 5.0 / 6.0 / 8.0 / 10 Larger welded pressure tube; watch family wall ceiling

Exact length, bevel, IGC, and sister-grade duals (1.4401, 1.4432, 1.4435, 1.4462) can share one enquiry. Catalogue size patterns are indicative; EN 10217-7 governs. SHH STEEL can produce and supply X2CrNiMo17-12-2 welded tube in this map when the mill path fits.

FAQ

What is EN 10217-7 1.4404 welded stainless steel tube used for?
EN 10217-7 1.4404 (X2CrNiMo17-12-2) is welded pressure tube for PED-oriented duties that need the austenitic chemistry story with a longitudinal mill seam. Typical service is coastal utilities, brine-adjacent process lines, pharmaceutical and food lines with chloride sanitiser exposure, and general chemical PED piping. Put EN 10217-7, the steel number, and TC1/TC2 on the purchase order so chemistry, weld route, delivery condition, and tests match Part 7 — not a seamless EN 10216-5 or ASTM tubing habit.
Is EN 10217-7 1.4404 the same as 316L under ASTM A269 or A312?
No. Commercial alias 316L may point at a similar chemistry idea, but EN 10217-7 is a European welded pressure-tube standard with its own tables, test categories, and delivery-condition symbols. ASTM A269 is nominal-wall general-service tubing; A312 is pipe. Order the standard that matches the drawing. See also A269 TP316L, A213 TP316L, SA213 TP316L, A312 TP316L, SA312 TP316L.
Does EN 10217-7 1.4404 include seamless tube?
No. EN 10217-7 covers welded tubes only. If the line specification requires seamless product, the correct European series is EN 10216-5 for seamless pressure stainless tubes. Live seamless sister page: EN 10216-5 1.4404. Site titles for this series always say Welded Tube; the body does not pretend Part 7 can supply seamless product.
What mechanical properties does EN 10217-7 require for 1.4404?
In the solution-annealed condition, public BSSA ambient tables for EN 10217-7 list Rp0.2 min 190 MPa, Rp1.0 min 225 MPa, Rm 490–690 MPa, and elongation 40% longitudinal / 30% transverse for walls within the family’s characterisation band. Confirm against the purchased edition; do not invent creep rupture or PREN digits.
1.4404 vs sister grades — which EN 10217-7 number should I buy?
Buy 1.4404 when the enquiry names this steel number or the duty matches low-carbon Mo-bearing austenitic for welded pressure tube in chloride-bearing and chemical PED service where 316L chemistry is the buyer’s default. Compare EN 10217-7 1.4401, EN 10217-7 1.4432, EN 10217-7 1.4435, EN 10217-7 1.4462 when carbon, Mo, stabilisation, nitrogen, or duplex strength points elsewhere. Design caution for this grade: 316L-family still has chloride SCC limits under tensile stress and temperature — duplex 1.4462 is often the next step when SCC governs
What delivery conditions are available for EN 10217-7 1.4404?
Delivery-condition symbols include W0, W1, W1A, W1R, W2, W2A, W2R, WCA, WCR, WG, and WP (bead-worked “b” suffix optional). Heat treatment is part of several symbols; mechanical tables assume solution-annealed (+AT) properties. Unless Option 5 is specified, the manufacturer chooses. SHH STEEL can produce and supply the common heat-treated descaled and cold-finished routes when the order locks Option 5 and any roughness scope.
What size range can SHH STEEL supply for EN 10217-7 1.4404?
SHH STEEL can produce and supply EN 10217-7 1.4404 in a typical enquiry band covering instrumentation through process OD with walls suited to longitudinal welded routes (~6–219 mm OD × 0.5–12.7 mm wall within family characterisation; other sizes by agreement), with EN 10204 3.1 documents. Larger or heavier sizes need agreement — send the OD × wall list for a firm availability answer. Widest commercial welded od×wall band in the mo austenitic family for en 10217-7.
TC1 or TC2 for EN 10217-7 1.4404?
Test category is mandatory order information and appears in marking. TC2 increases tensile sampling and raises the NDT / technological-test intensity on the weld seam relative to TC1. Choose TC2 when the PED file or purchaser specification demands the heavier regime. Leak-tightness applies to every tube in both categories.
Is the intergranular corrosion test mandatory for 1.4404?
No. IGC testing to EN ISO 3651-2 is Option 13. Tables mark resistance in the delivery condition for corrosion-resisting grades, but the test appears on the certificate only when ordered. Order Option 13 when the PED file or end-user specification requires a tested IGC result for 1.4404.
What documents come with SHH STEEL EN 10217-7 1.4404?
EN 10204 3.1 inspection documents report cast chemistry, delivery-condition / heat-treatment status, ambient tensile results, and leak-tightness / NDT statements. Option 21 upgrades to 3.2. Third-party inspection and PMI can be added on the order. Stencil carries EN 10217-7, 1.4404, size, cast, and test category.
How do I enquire for EN 10217-7 1.4404 with SHH STEEL?
Send EN 10217-7, steel number 1.4404 / X2CrNiMo17-12-2, TC1 or TC2, OD × wall list and lengths, delivery-condition symbol (or Option 5), and any Options (13 IGC, 15 leak-test method, 18 bevel, 19 exact length, 20 D4, 21 for 3.2). Add the service medium if grade selection is still open. SHH STEEL can produce and supply to that enquiry or recommend a sister number when the duty needs it.

Conclusion

EN 10217-7 1.4404 (X2CrNiMo17-12-2) is welded stainless pressure tube for PED-oriented service in the austenitic family — ordered by steel number, test category, and delivery-condition symbol, not by a shop alias alone. SHH STEEL can produce and supply 1.4404 with EN 10204 documentation, leak-tightness testing, and weld-seam NDT aligned to TC1 or TC2. For sizing, sister-grade advice, or a dual enquiry against seamless EN 10216-5 or live ASTM/ASME pages, contact admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X