EN 10217-7 1.4311 Welded Stainless Steel Tube | EN 10217-7 Stainless Steel - SHH STEEL

EN 10217-7 1.4311 Welded Stainless Steel Tube

EN 10217-7 1.4311 / X2CrNiN18-10 welded stainless pressure tube (304LN), austenitic, cast analysis per EN table, ambient Rp0.2 min 270 MPa, Rm 550–760, solution annealed 1000–1100 °C. SHH STEEL can produce and supply with EN 10204 3.1 MTCs, TC1/TC2 testing.
Grade
1.4311 / X2CrNiN18-10 (304LN — body alias)
Standard
EN 10217-7
Product form
Welded tube for pressure purposes (longitudinal arc/laser), solution annealed as required by delivery condition
Size
~6–219 mm OD × 0.5–12.7 mm wall within family characterisation; other sizes by agreement
Share:
Overview
Chemical Composition
Mechanical Properties
Welded Tube Manufacture
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is EN 10217-7 1.4311 Welded Stainless Steel Tube

Inside the EN 10217-7:2021 welded stainless pressure-tube list, 1.4311 / X2CrNiN18-10 is the austenitic grade purchasers pick when the duty matches this chemistry story. The standard covers circular welded tubes for pressure and corrosion-resisting purposes; it does not accept a bare “304LN” stamp as a substitute for steel number, delivery-condition symbol, or test category. Name EN 10217-7, 1.4311, TC1/TC2, and the options list on the purchase order so cast analysis, longitudinal weld manufacture, solution treatment where required, mechanical verification, and leak-tightness are unambiguous. Practical role: nitrogen-strengthened low-carbon 18-8 austenitic for welded pressure tube needing higher proof strength than 1.4307 without jumping to duplex.

SHH STEEL can produce and supply EN 10217-7 1.4311 welded stainless steel tube — longitudinally arc- or laser-welded from strip or plate on the standard’s manufacturing routes, solution annealed where the ordered delivery condition requires it, with EN 10204 3.1 inspection documents (3.2 under Option 21) reporting cast chemistry and ambient mechanical results against the ordered edition. Typical enquiry sizes cover same welded OD×wall conversation as 1.4307 with attention to higher tensile floors on the MTC. Browse the series hub at EN 10217-7.

When the stress calculation wants more than 1.4307’s Rp0.2 but the medium is still Mo-free aqueous service, 1.4311 is the EN 10217-7 nitrogen path. Typical welded pressure duties include higher-design-stress PED utilities, nitrogen-specified hygienic and process lines, and replacements where wall thickness was driven by 304L proof floors. Design caution: nitrogen raises strength but does not buy Mo-level pitting resistance — chloride duties still need 1.4404 or duplex when PREN-type thinking governs the medium Commercially the grade is often called 304LN; keep that name on the enquiry note and in the body, never as a substitute for steel number 1.4311 / X2CrNiN18-10 on the MTC. Sister numbers on this hub include EN 10217-7 1.4307, EN 10217-7 1.4301, EN 10217-7 1.4404, EN 10217-7 1.4429.4307, 1.4301, 1.4404, 1.4429.

Product-form discipline: order EN 10217-7 for welded 1.4311, EN 10216-5 for seamless. Dimensions lean on EN ISO 1127. Manufacture is longitudinal arc or laser from strip or plate per Table 1; spiral/helical is not invented as a listed Part 7 route in this series. Live seamless sister: EN 10216-5 1.4311. Related live ASTM/ASME anchors: A269 TP304L.

Chemical Composition of EN 10217-7 1.4311

Heat acceptance for 1.4311 starts with cast analysis to X2CrNiN18-10. Option 6 product analysis uses the standard’s permissible deviations. SHH STEEL documents real ladle results on EN 10204 3.1 and treats private catalogue windows as non-EN unless the purchaser agrees them separately.

The following cast analysis for X2CrNiN18-10 is taken from public BSSA EN 10217-7 data for steel number 1.4311. Maxima apply except where a range is shown. Verify against the ordered EN 10217-7:2021 text before release.

Element 1.4311 cast analysis (mass %)
Carbon (C) ≤0.030
Silicon (Si) ≤1.00
Manganese (Mn) ≤2.00
Phosphorus (P) ≤0.045
Sulfur (S) ≤0.015
Nitrogen (N) 0.12–0.22
Chromium (Cr) 17.0–19.5
Nickel (Ni) 8.5–11.5

Public BSSA EN 10217-7 chemistry underpins the 1.4311 / X2CrNiN18-10 table below. Cross-check is against the 2021 grade list framing. Scrap and finishing practice must still protect the austenitic property set — unlisted deliberate additions require agreement.

Mechanical Properties of EN 10217-7 1.4311

EN 10217-7 lists ambient tensile and ductility requirements for solution-annealed X2CrNiN18-10 (steel number 1.4311) in the austenitic table, covering walls up to about 60 mm by default. Both 0.2% and 1.0% proof stresses are specified. −196 °C impact data are available as characterisation; verification is an Option-driven act.

For 1.4311, the tensile and ductility floors below are BSSA EN 10217-7 ambient figures. Solution temperatures for X2CrNiN18-10 come from public EN stainless tables (UNCERTAIN against paid Part 7 footnotes). SHH STEEL will not inflate or swap those floors using another product standard’s numbers.

Property 1.4311 ambient (solution annealed +AT)
Rp0.2 min (MPa) 270
Rp1.0 min (MPa) 305
Rm (MPa) 550–760
A min % long / trans 35 / 30
IGC resistance (delivery) Yes (method A)
Solution annealing (public EN band) 1000–1100 °C — UNCERTAIN vs paid EN 10217-7:2021 footnote if diverges
Cooling water or air
Charpy sub-zero (transverse min J) 60 at -196 °C (Option to verify)

Mechanical source stack for 1.4311: BSSA EN 10217-7 ambient properties; public EN solution-anneal bands with UNCERTAIN paid-edition flag. Characterisation impact energies for X2CrNiN18-10 become certificate entries only through the relevant Options.

Welded Tube Manufacture for EN 10217-7 1.4311

Part 7 production of 1.4311 / X2CrNiN18-10 is a longitudinal weld story. Strip or plate is formed and closed by automatic arc or laser welding on a Table 1 route, with or without filler and with optional outside grind or bead work ahead of heat treatment. Everyday sizes run on strip; heavier walls use plate. Finished tubes exclude pre-forming strip-join welds. Helical manufacture is outside the listed routes — settle any non-standard seam in writing. Seamless pressure stainless is ordered under EN 10216-5, not under this welded page.

For austenitic 1.4311 (X2CrNiN18-10), mill seams are typically made without filler or with matching filler depending on route and wall; Options 3 and 4 cover inside-weld remelt or bead working when the purchaser wants a smoothed ID weld. Delivery condition symbols (Table 2) include W0, W1/W1A/W1R, W2/W2A/W2R, cold-finished WCA/WCR with recrystallized weld metal, and WG/WP ground or polished. Unless Option 5 is specified, selection is at the manufacturer’s discretion. SHH STEEL can produce and supply 1.4311 as W1A/W2A descaled or WCA/WCR cold-finished in the common pressure-tube band, and as WG/WP when roughness is agreed. match nitrogen-bearing or overlying austenitic fillers; avoid procedures that dilute nitrogen out of the weld metal without agreement

Do not leave test category blank on 1.4311. TC1 and TC2 change NDT and tensile intensity on the longitudinal weld; leak-tightness still applies to each tube, and Option 15 can prescribe how. SHH STEEL records executed weld route and delivery symbol against the X2CrNiN18-10 heat.

Dimensions and Tolerances for EN 10217-7 1.4311

Buyers order 1.4311 (X2CrNiN18-10) on outside diameter and wall thickness. EN ISO 1127 preferred sizes and stainless densities apply. EN 10217-7 tolerance classes (Option 20 → D4) govern diameter and wall; ovality and eccentricity remain inside those envelopes, and abutting-edge radial offset at the weld is limited per public text.

Exact-length Option 19 and bevel Option 18 (wall ≥ 3.2 mm) are standard extras. For 304LN-class welded pressure tube needing tighter OD, WCA/WCR is usually discussed alongside W1A/W2A. SHH STEEL locks OD × wall, class, and symbol on the 1.4311 order prior to welding.

Route / condition Typical use Notes
W1 / W1A / W1R Hot-rolled starting flat product Descaled or bright-annealed per symbol
W2 / W2A / W2R Cold-rolled starting flat product Smoother OD than W1 family except at weld
WCA / WCR Cold finished ≥20% after weld Recrystallized weld metal; OD often ≤168.3 mm
WG / WP Ground / polished Agree ID/OD scope and grit at enquiry

Release of EN 10217-7 1.4311 includes confirmation that OD × wall sit inside the purchased class for X2CrNiN18-10. Straightness and end condition are inspected to the standard; cold-finished routes are recommended when D4 is specified. SHH STEEL confirms OD × wall and the selected EN ISO 1127 / Part 7 tolerance class for 1.4311 / X2CrNiN18-10 on the inspection document rather than assuming mid-tolerance catalogue values.

Equivalent Grades for EN 10217-7 1.4311

Steel number 1.4311 with name X2CrNiN18-10 is what EN 10217-7 stamps on welded pressure tube of this analysis. Alias 304LN is commercial language. Treat ASTM/ASME lookalikes and EN 10216-5 seamless pages as related references — verify before dual-marking or substituting.

Bill-of-materials writers sometimes list 304LN next to EN and ASTM numbers interchangeably. For this product, steel number 1.4311 with name X2CrNiN18-10 under EN 10217-7 is the welded acceptance path; confirm any dual mark against both mechanical tables before release to fabrication.

Reference Designation Note
EN 10217-7 1.4311 / X2CrNiN18-10 This product standard (welded pressure tube)
EN steel name X2CrNiN18-10 EN 10027-1 designation used in body and marking
Commercial alias (body only) 304LN Not a substitute for the steel number on the MTC
EN 10216-5 (seamless sister) 1.4311 Related live page — different product form (seamless)
A269 TP304L A269 TP304L Related live page — different product standard

Inside this welded series, compare EN 10217-7 1.4307, EN 10217-7 1.4301, EN 10217-7 1.4404, EN 10217-7 1.4429. Hub: EN 10217-7. Seamless sister: EN 10216-5 1.4311. Live cross-standard anchors: A269 TP304L.

Heat Treatment and Delivery Condition for EN 10217-7 1.4311

Choose the Table 2 symbol for 1.4311 with heat treatment in mind. W1A/W2A, cold-finished WCA/WCR, and bright-annealed W1R/W2R all imply treated routes; mechanical acceptance for X2CrNiN18-10 is written for solution-annealed (+AT) tube. For X2CrNiN18-10 under steel number 1.4311, keep Option 5 in mind when the delivery-condition symbol must be contractual, and reconcile the certificate wording with the solution-annealing practice actually used on the welded tube before releasing the PED file.

Reference solution window for 1.4311: 1000–1100 °C with water or air cooling, drawn from public EN stainless tables and flagged UNCERTAIN vs paid Part 7 notes. Surface finish remains a Table 2 / Option 5 decision after heat treatment of X2CrNiN18-10. For X2CrNiN18-10 under steel number 1.4311, keep Option 5 in mind when the delivery-condition symbol must be contractual, and reconcile the certificate wording with the solution-annealing practice actually used on the welded tube before releasing the PED file.

Item 1.4311
Solution annealing band (public) 1000–1100 °C (UNCERTAIN vs paid Part 7 footnote)
Cooling water or air
Delivery condition symbols W0 / W1 / W1A / W1R / W2 / W2A / W2R / WCA / WCR / WG / WP (Option 5 to specify)
Inspection document EN 10204 3.1 default; 3.2 under Option 21

Delivery-condition control for 1.4311 means more than a furnace ticket: SHH STEEL records the symbol, the heat treatment implied for X2CrNiN18-10, and cold-finished weld recrystallization status when WCA/WCR applies, then ships only material that matches that record. For X2CrNiN18-10 under steel number 1.4311, keep Option 5 in mind when the delivery-condition symbol must be contractual, and reconcile the certificate wording with the solution-annealing practice actually used on the welded tube before releasing the PED file.

Corrosion Resistance of EN 10217-7 1.4311

Choose 1.4311 (X2CrNiN18-10) when welded PED tubing must carry this corrosion story: low carbon plus nitrogen; aqueous resistance similar to 304L-family with improved mechanical floors from interstitial strengthening. Delivery-condition IGC resistance is characterised to EN ISO 3651-2 methods in the Part 7 tables, but a tested IGC result still requires Option 13 on the order.

If fabrication will leave 1.4311 as-welded in a corrosive medium, re-read the carbon/stabilisation/Mo story for X2CrNiN18-10 and the caution on this pack. Sister options EN 10217-7 1.4307, EN 10217-7 1.4301, EN 10217-7 1.4404, EN 10217-7 1.4429 exist for a reason. PREN invention is outside SHH STEEL’s EN 10217-7 acceptance practice.

Applications of EN 10217-7 1.4311 Tube

Applications for steel number 1.4311 / X2CrNiN18-10 cluster around welded PED service that tolerates a mill seam: higher-design-stress PED utilities, nitrogen-specified hygienic and process lines, and replacements where wall thickness was driven by 304L proof floors. Delivery condition and test category on the order decide how that tube is finished and inspected before it reaches the spool.

Skip 1.4311 when the specification locks seamless product (EN 10216-5 — see EN 10216-5 1.4311), when ASTM A269/A312 text is the only acceptance language, or when corrosion/strength clearly points at another family. SHH STEEL can produce and supply X2CrNiN18-10 welded tube in the enquiry band and will redirect to a sister or live ASTM/ASME page when that is wiser. Related live pages: A269 TP304L.

Weldability of EN 10217-7 1.4311

Mill welding of EN 10217-7 1.4311 is the longitudinal arc/laser seam on the ordered Table 1 route; field or shop welding is a separate PED joint design. Filler and procedure choices track the austenitic chemistry of X2CrNiN18-10. Practical note: match nitrogen-bearing or overlying austenitic fillers; avoid procedures that dilute nitrogen out of the weld metal without agreement

Mill weldability of 1.4311 is proven on the Table 1 route; fabricator weldability is proven on the WPS. Keep those scopes apart. SHH STEEL certifies X2CrNiN18-10 mill tube to the ordered delivery condition and inspection Options, and leaves joint design — including as-welded service limits — with the PED responsible party.

Surface Finishes for EN 10217-7 1.4311

W1A/W2A descaled, W1R/W2R/WCR bright-annealed, and WG/WP ground or polished are the finish vocabulary for 1.4311. Write roughness when WP/WG is wanted; do not assume a grit from a brochure photo of X2CrNiN18-10. Carbon-steel banding on stainless is rejected in SHH STEEL packing rules because free-iron stains on 304LN are expensive to remove and easy to prevent at the dock.

Anything beyond Table 2 surface language needs writing: Ra, EP, films, capped cleanliness. SHH STEEL can produce and supply finishes it can report for EN 10217-7 1.4311; unmeasured grit marketing is not offered for X2CrNiN18-10, and commercial 304LN habits do not override that discipline.

If the drawing shows a hygienic OD note without EN delivery language, translate it into W1R/W2R, WCR, or WP with criteria before releasing 1.4311. SHH STEEL will help map that note onto a measurable finish for X2CrNiN18-10 instead of guessing what the last fabricator accepted on unlabeled 304LN tube.

Inspection and Testing for EN 10217-7 1.4311

Baseline Part 7 inspection for 1.4311: cast analysis, room-temperature tensile at the ordered test-category rate, technological tests, full leak-tightness coverage, plus dimensional/visual/ID work on X2CrNiN18-10. Hydrostatic or eddy-current leak testing may be locked with Option 15. Keep TC1/TC2, Option 13 IGC, and any impact Options visible on the 1.4311 purchase order so X2CrNiN18-10 inspection planning matches the PED file before weld slots are locked.

TC2, Option 13 IGC, and impact Options are how purchasers thicken the 1.4311 inspection story beyond baseline leak-tightness and tensile. SHH STEEL documents chemistry, heat treatment, tensile, and NDT/leak results for X2CrNiN18-10 and will not delete mandatory tests to chase a shorter promise date.

Dual-certification enquiries for 1.4311 must list every standard’s test extras up front. SHH STEEL maps EN 10217-7 obligations for X2CrNiN18-10 first, then adds agreed ASTM/ASME layers without pretending one test covers both.

Packaging and Shipping for EN 10217-7 1.4311

Dispatch packing on EN 10217-7 1.4311 covers mechanical protection and stainless hygiene. Caps or plugs close the ends, bundles are size-sorted, and waterproof wrap covers long sea legs. Bright-annealed and polished OD (W1R/W2R, WCR, WP) take sleeve or paper wrap against transit galling; descaled W1A/W2A utility tube still needs clean supports under the longitudinal seam. Contact materials exclude bare carbon steel so X2CrNiN18-10 OD — commercially still discussed as 304LN — does not pick up rust blooms in transit that complicate PED receiving inspection.

Marking discipline for 1.4311: standard, steel number or X2CrNiN18-10, size, cast, TC1/TC2, inspection marks. Delivery symbols follow manufacturer practice unless Option 5 demands them. SHH STEEL verifies the marking clause on the 304LN order prior to shipment. SHH STEEL treats packing and marking for EN 10217-7 1.4311 / X2CrNiN18-10 as part of product conformity, not as a warehouse afterthought, so the PED receiving inspection sees protected ends, clean contact materials, and stencil text that matches the certificate.

Ocean and road packs for 1.4311 keep heat identity visible at bundle level. Bevelled and exact-length tube is capped and segregated. SHH STEEL closes packaging only after the order’s packing and marking lines are satisfied for this 304LN grade. SHH STEEL treats packing and marking for EN 10217-7 1.4311 / X2CrNiN18-10 as part of product conformity, not as a warehouse afterthought, so the PED receiving inspection sees protected ends, clean contact materials, and stencil text that matches the certificate.

Why Choose SHH STEEL

SHH STEEL can produce and supply 1.4311 welded stainless pressure tube with matching heat treatment and TC1/TC2 documentation for X2CrNiN18-10. The commercial alias 304LN may appear in body text; it does not replace the steel number on the certificate, and sister-standard tensile floors stay off this Part 7 document.

Use LINKPLACE1.4307, LINKPLACE1.4301, LINKPLACE1.4404, LINKPLACE1.4429 as the short-list when 1.4311 is borderline. Remember: nitrogen raises strength but does not buy Mo-level pitting resistance — chloride duties still need LINKPLACE1.4404 or duplex when PREN-type thinking governs the medium The PED file needs the right steel number more than it needs a fast yes Linked sisters on this hub: EN 10217-7 1.4307, EN 10217-7 1.4301, EN 10217-7 1.4404, EN 10217-7 1.4429. Live ASTM/ASME anchors: A269 TP304L.

Supply Capability

SHH STEEL can produce and supply 1.4311 welded stainless pressure tube under EN 10217-7 with the documents and tests your enquiry lists. Capability plus Stock / Available sizes below are the sizing scratchpad for X2CrNiN18-10. Same welded od×wall conversation as 1.4307 with attention to higher tensile floors on the mtc.

Item SHH STEEL capability for 1.4311
Standard EN 10217-7
Grade 1.4311 / X2CrNiN18-10
Product form Welded tube for pressure purposes (longitudinal arc/laser), solution annealed as required by delivery condition
Delivery condition W0 / W1 / W1A / W1R / W2 / W2A / W2R / WCA / WCR / WG / WP (Option 5 to lock)
Typical size band ~6–219 mm OD × 0.5–12.7 mm wall within family characterisation; other sizes by agreement
Testing TC1 or TC2; leak-tightness each tube; weld-seam NDT per category / options
Documents EN 10204 3.1 (3.2 Option 21); third-party inspection on request

Stock / Available sizes

The Stock / Available sizes block for 1.4311 is a planning aid. Actual commitment waits on X2CrNiN18-10 melt/strip position and the ordered W-symbol finishing path. Send sizes, TC1/TC2, and delivery condition to firm it up.

OD (mm) Typical walls (mm) Notes
12 / 14 / 16 / 19 / 21.3 / 25 1.0 / 1.5 / 2.0 / 2.5 Instrument / hygienic; often WCA/WCR or W2R
26.9 / 33.7 / 38 / 42.4 / 48.3 1.5 / 2.0 / 2.5 / 3.0 / 4.0 Process and utility welded pressure tube
60.3 / 76.1 / 88.9 / 114.3 2.0 / 3.0 / 4.0 / 5.0 / 6.0 Utility and process; lock W1A/W2A vs WCA
141.3 / 168.3 / 219.1 3.0 / 4.0 / 5.0 / 6.0 / 8.0 / 10 Larger welded pressure tube; watch family wall ceiling

Option-driven extras and sister comparisons (1.4307, 1.4301, 1.4404, 1.4429) belong on the enquiry. Size rows are typical, not promised stock. SHH STEEL can produce and supply EN 10217-7 1.4311 across this map when X2CrNiN18-10 feedstock and weld capacity agree.

FAQ

What is EN 10217-7 1.4311 welded stainless steel tube used for?
EN 10217-7 1.4311 (X2CrNiN18-10) is welded pressure tube for PED-oriented duties that need the austenitic chemistry story with a longitudinal mill seam. Typical service is higher-design-stress PED utilities, nitrogen-specified hygienic and process lines, and replacements where wall thickness was driven by 304L proof floors. Put EN 10217-7, the steel number, and TC1/TC2 on the purchase order so chemistry, weld route, delivery condition, and tests match Part 7 — not a seamless EN 10216-5 or ASTM tubing habit.
Is EN 10217-7 1.4311 the same as 304LN under ASTM A269 or A312?
No. Commercial alias 304LN may point at a similar chemistry idea, but EN 10217-7 is a European welded pressure-tube standard with its own tables, test categories, and delivery-condition symbols. ASTM A269 is nominal-wall general-service tubing; A312 is pipe. Order the standard that matches the drawing. See also A269 TP304L.
Does EN 10217-7 1.4311 include seamless tube?
No. EN 10217-7 covers welded tubes only. If the line specification requires seamless product, the correct European series is EN 10216-5 for seamless pressure stainless tubes. Live seamless sister page: EN 10216-5 1.4311. Site titles for this series always say Welded Tube; the body does not pretend Part 7 can supply seamless product.
What mechanical properties does EN 10217-7 require for 1.4311?
In the solution-annealed condition, public BSSA ambient tables for EN 10217-7 list Rp0.2 min 270 MPa, Rp1.0 min 305 MPa, Rm 550–760 MPa, and elongation 35% longitudinal / 30% transverse for walls within the family’s characterisation band. Confirm against the purchased edition; do not invent creep rupture or PREN digits.
1.4311 vs sister grades — which EN 10217-7 number should I buy?
Buy 1.4311 when the enquiry names this steel number or the duty matches nitrogen-strengthened low-carbon 18-8 austenitic for welded pressure tube needing higher proof strength than 1.4307 without jumping to duplex. Compare EN 10217-7 1.4307, EN 10217-7 1.4301, EN 10217-7 1.4404, EN 10217-7 1.4429 when carbon, Mo, stabilisation, nitrogen, or duplex strength points elsewhere. Design caution for this grade: nitrogen raises strength but does not buy Mo-level pitting resistance — chloride duties still need 1.4404 or duplex when PREN-type thinking governs the medium
What delivery conditions are available for EN 10217-7 1.4311?
Delivery-condition symbols include W0, W1, W1A, W1R, W2, W2A, W2R, WCA, WCR, WG, and WP (bead-worked “b” suffix optional). Heat treatment is part of several symbols; mechanical tables assume solution-annealed (+AT) properties. Unless Option 5 is specified, the manufacturer chooses. SHH STEEL can produce and supply the common heat-treated descaled and cold-finished routes when the order locks Option 5 and any roughness scope.
What size range can SHH STEEL supply for EN 10217-7 1.4311?
SHH STEEL can produce and supply EN 10217-7 1.4311 in a typical enquiry band covering instrumentation through process OD with walls suited to longitudinal welded routes (~6–219 mm OD × 0.5–12.7 mm wall within family characterisation; other sizes by agreement), with EN 10204 3.1 documents. Larger or heavier sizes need agreement — send the OD × wall list for a firm availability answer. Same welded od×wall conversation as 1.4307 with attention to higher tensile floors on the mtc.
TC1 or TC2 for EN 10217-7 1.4311?
Test category is mandatory order information and appears in marking. TC2 increases tensile sampling and raises the NDT / technological-test intensity on the weld seam relative to TC1. Choose TC2 when the PED file or purchaser specification demands the heavier regime. Leak-tightness applies to every tube in both categories.
Is the intergranular corrosion test mandatory for 1.4311?
No. IGC testing to EN ISO 3651-2 is Option 13. Tables mark resistance in the delivery condition for corrosion-resisting grades, but the test appears on the certificate only when ordered. Order Option 13 when the PED file or end-user specification requires a tested IGC result for 1.4311.
What documents come with SHH STEEL EN 10217-7 1.4311?
EN 10204 3.1 inspection documents report cast chemistry, delivery-condition / heat-treatment status, ambient tensile results, and leak-tightness / NDT statements. Option 21 upgrades to 3.2. Third-party inspection and PMI can be added on the order. Stencil carries EN 10217-7, 1.4311, size, cast, and test category.
How do I enquire for EN 10217-7 1.4311 with SHH STEEL?
Send EN 10217-7, steel number 1.4311 / X2CrNiN18-10, TC1 or TC2, OD × wall list and lengths, delivery-condition symbol (or Option 5), and any Options (13 IGC, 15 leak-test method, 18 bevel, 19 exact length, 20 D4, 21 for 3.2). Add the service medium if grade selection is still open. SHH STEEL can produce and supply to that enquiry or recommend a sister number when the duty needs it.

Conclusion

EN 10217-7 1.4311 (X2CrNiN18-10) is welded stainless pressure tube for PED-oriented service in the austenitic family — ordered by steel number, test category, and delivery-condition symbol, not by a shop alias alone. SHH STEEL can produce and supply 1.4311 with EN 10204 documentation, leak-tightness testing, and weld-seam NDT aligned to TC1 or TC2. For sizing, sister-grade advice, or a dual enquiry against seamless EN 10216-5 or live ASTM/ASME pages, contact admin@steelspecs.com.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X