EN 10025-2 S235JR H-Beam

EN 10025-2 S235JR H-beam is a non-alloy structural section (1.0038) with 235 MPa minimum yield up to 16 mm and 27 J impact at +20 °C. Sizes follow the HEA, HEB and IPE series under EN 10365, with tolerances under EN 10034. SHH STEEL reviews grade, size and certificate requirements before quoting.
Keywords
EN 10025-2 S235JR H-Beam, S235JR HEA, S235JR HEB, S235JR IPE, 1.0038 structural H-beam
Equivalent Grades:
Near-equivalents only, not automatic substitutes: S235J0/J2; Q235B; ASTM A36; JIS SS400.
Share:
General Description
Material Specification
Available Sizes of S235JR H-Beam
Chemical Composition
Carbon Equivalent
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why Source S235JR H-Beams from SHH STEEL
FAQ
Conclusion

What is EN 10025-2 S235JR H-Beam?

EN 10025-2 S235JR H-beam is a hot-rolled I or H section whose material grade is S235JR (steel number 1.0038) under EN 10025-2 and whose shape, dimensions and tolerances are ordered to EN 10365 and EN 10034. S stands for structural steel, 235 is the minimum yield strength in MPa for the thinnest tabulated thickness band, and JR is the quality, which carries a 27 J Charpy V-notch requirement at +20 °C.

This page covers the rolled section, not plate. The same grade in plate form is listed separately as EN 10025-2 S235JR steel plate. For long products, tensile and impact tests are normally longitudinal unless the order says otherwise; plate sampling is a different convention. The plate page is not a substitute data sheet for H-beams.

These beams are filed under EN 10025-2 steel beam profiles in the steel beam profiles category of steel structural profiles. The usual European size series are HE A (HEA), HE B (HEB) and IPE. HE M (HEM) and British UB or UC sections may be furnished when they are specified and certified; they are not treated here as interchangeable with HEA or IPE of a similar nominal depth. The published S355JR H-beam page is the 355 MPa sister in the same family, not a data sheet for S235JR.

S235JR is a non-alloy structural steel for building frames, workshops and ordinary fabrication where a +20 °C impact quality is accepted. It is not a 355 MPa grade, not a weathering steel, and not a pressure-vessel or nuclear safety material. If an enquiry only says “S235 H-beam,” the quality letters and the dimensional standard still need to be confirmed.

Material, Dimensions and Tolerances for S235JR Sections

Three documents should appear, separately, on the purchase order and on the inspection certificate:

  • EN 10025-2 is the material standard for non-alloy structural steels. This article uses ladle-analysis, carbon-equivalent and tensile values for S235JR long products from EN 10025-2:2019. The edition named on the order governs acceptance.
  • EN 10365 is the dimensional standard for hot-rolled I and H sections, including IPE and the HE A, HE B and HE M family. The numbers in the size tables below are reference dimensions and theoretical masses for the standard HE A, HE B and IPE series, not a rolling list for a particular mill.
  • EN 10034 is the tolerance standard for I and H sections. It covers depth, width, thickness, out-of-square, web off-centre, straightness and related shape and mass tolerances. Surface condition for sections is commonly specified to EN 10163-3; the class should be confirmed when a tighter finish is required.

A mill may roll a European HE or IPE shape and certify a different material standard, or roll a metric H or W-shape and certify S235JR, if that combination is in its programme and is fully documented. Do not treat “S235JR H-beam” as if it automatically meant an HEA section, and do not treat a Chinese HW or an American W of a similar nominal depth as the same section.

S235JR H-Beam Sizes: HEA, HEB, IPE, UB and UC Reference Tables

The tables give designation, depth h, width b, web thickness tw, flange thickness tf, root radius r, cross-sectional area A and theoretical mass per metre for the standard HE A, HE B and IPE series, consistent with the established EN 10365 series. They are reference dimensions for identification and estimating, not a claim that every size is produced in S235JR. Mid-range HEA, HEB and IPE sizes are the usual enquiry core; the lightest IPE rows, HE 1000 and less common variants should be confirmed size by size.

Two designation habits are in use. EN writing uses a space and a letter after the size number: HE 200 A, HE 200 B, HE 200 M. Trade writing often compresses this to HEA 200, HEB 200 and HEM 200. They name the same standard sections. IPE uses the series letters plus the nominal depth, for example IPE 300. The nominal depth is not always the actual depth: HE 300 A / HEA 300 has h = 290 mm, while HE 300 B / HEB 300 has h = 300 mm. IPE sections are narrower parallel-flange I-beams; IPE 300 is 300 × 150 mm, not 300 × 300 mm.

Apply the EN 10025-2 thickness band that matches the governing thickness of the ordered size, usually the flange. The headline 235 MPa yield applies only up to 16 mm. Many mid-range flanges sit in the 16–40 mm band, where the minimum yield is 225 MPa. For sections with nominal thickness greater than 100 mm, the mechanical values are subject to agreement.

HE A (HEA) series

Wide-flange European H-sections, 24 sizes from HE 100 A to HE 1000 A.

Swipe horizontally to view all dimensions.

Designation h (mm) b (mm) tw (mm) tf (mm) r (mm) A (cm²) Mass (kg/m)
HE 100 A 96 100 5 8 12 21.2 16.7
HE 120 A 114 120 5 8 12 25.3 19.9
HE 140 A 133 140 5.5 8.5 12 31.4 24.7
HE 160 A 152 160 6 9 15 38.8 30.4
HE 180 A 171 180 6 9.5 15 45.3 35.5
HE 200 A 190 200 6.5 10 18 53.8 42.3
HE 220 A 210 220 7 11 18 64.3 50.5
HE 240 A 230 240 7.5 12 21 76.8 60.3
HE 260 A 250 260 7.5 12.5 24 86.8 68.2
HE 280 A 270 280 8 13 24 97.3 76.4
HE 300 A 290 300 8.5 14 27 112.5 88.3
HE 320 A 310 300 9 15.5 27 124.4 97.6
HE 340 A 330 300 9.5 16.5 27 133.5 105
HE 360 A 350 300 10 17.5 27 142.8 112
HE 400 A 390 300 11 19 27 159.0 125
HE 450 A 440 300 11.5 21 27 178.0 140
HE 500 A 490 300 12 23 27 197.5 155
HE 550 A 540 300 12.5 24 27 211.8 166
HE 600 A 590 300 13 25 27 226.5 178
HE 650 A 640 300 13.5 26 27 241.6 190
HE 700 A 690 300 14.5 27 27 260.5 204
HE 800 A 790 300 15 28 30 285.8 224
HE 900 A 890 300 16 30 30 320.5 252
HE 1000 A 990 300 16.5 31 30 346.8 272

HE B (HEB) series

Heavier-flange European H-sections, 24 sizes from HE 100 B to HE 1000 B.

Swipe horizontally to view all dimensions.

Designation h (mm) b (mm) tw (mm) tf (mm) r (mm) A (cm²) Mass (kg/m)
HE 100 B 100 100 6 10 12 26.0 20.4
HE 120 B 120 120 6.5 11 12 34.0 26.7
HE 140 B 140 140 7 12 12 43.0 33.7
HE 160 B 160 160 8 13 15 54.3 42.6
HE 180 B 180 180 8.5 14 15 65.3 51.2
HE 200 B 200 200 9 15 18 78.1 61.3
HE 220 B 220 220 9.5 16 18 91.0 71.5
HE 240 B 240 240 10 17 21 106.0 83.2
HE 260 B 260 260 10 17.5 24 118.4 93.0
HE 280 B 280 280 10.5 18 24 131.4 103
HE 300 B 300 300 11 19 27 149.1 117
HE 320 B 320 300 11.5 20.5 27 161.3 127
HE 340 B 340 300 12 21.5 27 170.9 134
HE 360 B 360 300 12.5 22.5 27 180.6 142
HE 400 B 400 300 13.5 24 27 197.8 155
HE 450 B 450 300 14 26 27 218.0 171
HE 500 B 500 300 14.5 28 27 238.6 187
HE 550 B 550 300 15 29 27 254.1 199
HE 600 B 600 300 15.5 30 27 270.0 212
HE 650 B 650 300 16 31 27 286.3 225
HE 700 B 700 300 17 32 27 306.4 241
HE 800 B 800 300 17.5 33 30 334.2 262
HE 900 B 900 300 18.5 35 30 371.3 291
HE 1000 B 1000 300 19 36 30 400.0 314

IPE series

Parallel-flange I-beams, 18 sizes from IPE 80 to IPE 600.

Swipe horizontally to view all dimensions.

Designation h (mm) b (mm) tw (mm) tf (mm) r (mm) A (cm²) Mass (kg/m)
IPE 80 80.0 46.0 3.8 5.2 5 7.6 6.0
IPE 100 100.0 55.0 4.1 5.7 7 10.3 8.1
IPE 120 120.0 64.0 4.4 6.3 7 13.2 10.4
IPE 140 140.0 73.0 4.7 6.9 7 16.4 12.9
IPE 160 160.0 82.0 5.0 7.4 9 20.1 15.8
IPE 180 180.0 91.0 5.3 8.0 9 23.9 18.8
IPE 200 200.0 100.0 5.6 8.5 12 28.5 22.4
IPE 220 220.0 110.0 5.9 9.2 12 33.4 26.2
IPE 240 240.0 120.0 6.2 9.8 15 39.1 30.7
IPE 270 270.0 135.0 6.6 10.2 15 45.9 36.1
IPE 300 300.0 150.0 7.1 10.7 15 53.8 42.2
IPE 330 330.0 160.0 7.5 11.5 18 62.6 49.1
IPE 360 360.0 170.0 8.0 12.7 18 72.7 57.1
IPE 400 400.0 180.0 8.6 13.5 21 84.5 66.3
IPE 450 450.0 190.0 9.4 14.6 21 98.8 77.6
IPE 500 500.0 200.0 10.2 16.0 21 115.5 90.7
IPE 550 550.0 210.0 11.1 17.2 24 134.4 106
IPE 600 600.0 220.0 12.0 19.0 24 156.0 122

Typical mill-programme universal beams (UB) and universal columns (UC) commonly supplied in S235JR are tabulated below. Designations follow the established EN 10365 / British universal naming (for example UB 610 × 229 × 125). The rows are a commonly supplied standard mill series, not a claim that every official EN 10365:2017 row has been reproduced or that any one mill rolls the full list in S235JR. Historic or additional depths can be reviewed on enquiry; they are not silently added to these tables. Masses are theoretical catalogue figures for identification, estimating and drawing work.

Universal beams (UB)

Swipe horizontally to view all dimensions.

Designation Mass (kg/m) h (mm) b (mm) tw (mm) tf (mm) r (mm)
UB 1016 × 305 × 584 584 1056 314 36 64 30
UB 1016 × 305 × 494 494 1036 309 31 54 30
UB 1016 × 305 × 438 438 1026 305 26.9 49 30
UB 1016 × 305 × 415 415 1020 304 26 46 30
UB 1016 × 305 × 393 393 1016 303 24.4 43.9 30
UB 1016 × 305 × 350 350 1008 302 21.1 40 30
UB 1016 × 305 × 314 314 1000 300 19.1 35.9 30
UB 1016 × 305 × 272 272 990 300 16.5 31 30
UB 1016 × 305 × 249 249 980 300 16.5 26 30
UB 1016 × 305 × 222 222 970 300 16 21.1 30
UB 914 × 305 × 576 576 993 322 36.1 65 20
UB 914 × 305 × 521 521 981 319 33 58.9 20
UB 914 × 305 × 474 474 971 316 30 54.1 20
UB 914 × 305 × 425 425 961 313 26.9 49 20
UB 914 × 305 × 381 381 951 310 24.4 43.9 20
UB 914 × 305 × 345 345 943 308 22.1 39.9 20
UB 914 × 305 × 313 313 932 309 21.1 34.5 20
UB 914 × 305 × 289 289 926.6 307.7 19.5 32 20
UB 914 × 305 × 271 271 923 307 18.4 30 20
UB 914 × 305 × 253 253 918.4 305.5 17.3 27.9 20
UB 914 × 305 × 238 238 915 305 16.5 25.9 20
UB 914 × 305 × 224 224 910.4 304.1 15.9 23.9 20
UB 914 × 305 × 201 201 903 303.3 15.1 20.2 20
UB 838 × 292 × 226 226 850.9 293.8 16.1 26.8 20
UB 838 × 292 × 194 194 840.7 292.4 14.7 21.7 20
UB 838 × 292 × 176 176 834.9 291.7 14 18.8 20
UB 762 × 267 × 197 197 769.8 268 15.6 25.4 20
UB 762 × 267 × 173 173 762.2 266.7 14.3 21.6 20
UB 762 × 267 × 147 147 754 265.2 12.8 17.5 20
UB 762 × 267 × 134 134 750 264.4 12 15.5 20
UB 686 × 254 × 170 170 692.9 255.8 14.5 23.7 20
UB 686 × 254 × 152 152 687.5 254.5 13.2 21 20
UB 686 × 254 × 140 140 683.5 253.7 12.4 19 20
UB 686 × 254 × 125 125 677.9 253 11.7 16.2 20
UB 610 × 305 × 238 238 635.8 311.4 18.4 31.4 20
UB 610 × 305 × 179 179 620.2 307.1 14.1 23.6 20
UB 610 × 305 × 149 149 612.4 304.8 11.8 19.7 20
UB 610 × 229 × 140 140 617.2 230.2 13.1 22.1 20
UB 610 × 229 × 125 125 612.2 229 11.9 19.6 20
UB 610 × 229 × 113 113 607.6 228.2 11.1 17.3 20
UB 610 × 229 × 101 101 602.6 227.6 10.5 14.8 20
UB 533 × 210 × 122 122 544.5 211.9 12.7 21.3 13
UB 533 × 210 × 109 109 539.5 210.8 11.6 18.8 13
UB 533 × 210 × 101 101 536.7 210 10.8 17.4 13
UB 533 × 210 × 92 92.1 533.1 209.3 10.1 15.6 13
UB 533 × 210 × 82 82.2 528.3 208.8 9.6 13.2 13
UB 457 × 191 × 98 98.3 467.2 192.8 11.4 19.6 10
UB 457 × 191 × 89 89.3 463.4 191.9 10.5 17.7 10
UB 457 × 191 × 82 82 460 191.3 9.9 16 10
UB 457 × 191 × 74 74.3 457 190.4 9 14.5 10
UB 457 × 191 × 67 67.1 453.4 189.9 8.5 12.7 10
UB 457 × 152 × 82 82.1 465.8 155.3 10.5 18.9 10
UB 457 × 152 × 74 74.2 462 154.4 9.6 17 10
UB 457 × 152 × 67 67.2 458 153.8 9 15 10
UB 457 × 152 × 60 59.8 454.6 152.9 8.1 13.3 10
UB 457 × 152 × 52 52.3 449.8 152.4 7.6 10.9 10
UB 406 × 178 × 74 74.2 412.8 179.5 9.5 16 10
UB 406 × 178 × 67 67.1 409.4 178.8 8.8 14.3 10
UB 406 × 178 × 60 60.1 406.4 177.9 7.9 12.8 10
UB 406 × 178 × 54 54.1 402.6 177.7 7.7 10.9 10
UB 406 × 140 × 46 46 403.2 142.2 6.8 11.2 10
UB 406 × 140 × 39 39 398 141.8 6.4 8.6 10
UB 356 × 171 × 67 67.1 363.4 173.2 9.1 15.7 10
UB 356 × 171 × 57 57 358 172.2 8.1 13 10
UB 356 × 171 × 51 51 355 171.5 7.4 11.5 10
UB 356 × 171 × 45 45 351.4 171.1 7 9.7 10
UB 356 × 127 × 39 39.1 353.4 126 6.6 10.7 10
UB 356 × 127 × 33 33.1 349 125.4 6 8.5 10
UB 305 × 165 × 54 54 310.4 166.9 7.9 13.7 9
UB 305 × 165 × 46 46.1 306.6 165.7 6.7 11.8 9
UB 305 × 165 × 40 40.3 303.4 165 6 10.2 9
UB 305 × 127 × 48 48.1 311 125.3 9 14 9
UB 305 × 127 × 42 41.9 307.2 124.3 8 12.1 9
UB 305 × 127 × 37 37 304.4 123.4 7.1 10.7 9
UB 305 × 102 × 33 32.8 312.7 102.4 6.6 10.8 8
UB 305 × 102 × 28 28.2 308.7 101.8 6 8.8 8
UB 305 × 102 × 25 24.8 305.1 101.6 5.8 7 8
UB 254 × 146 × 43 43 259.6 147.3 7.2 12.7 8
UB 254 × 146 × 37 37 256 146.4 6.3 10.9 8
UB 254 × 146 × 31 31.1 251.4 146.1 6 8.6 8
UB 254 × 102 × 28 28.3 260.4 102.2 6.3 10 8
UB 254 × 102 × 25 25.2 257.2 101.9 6 8.4 8
UB 254 × 102 × 22 22 254 101.6 5.7 6.8 8
UB 203 × 133 × 30 30 206.8 133.9 6.4 9.6 8
UB 203 × 133 × 25 25.1 203.2 133.2 5.7 7.8 8
UB 203 × 102 × 23 23.1 203.2 101.8 5.4 9.3 8
UB 178 × 102 × 19 19 177.8 101.2 4.8 7.9 8
UB 152 × 89 × 16 16 152.4 88.7 4.5 7.7 8
UB 127 × 76 × 13 13 127 76 4 7.6 8

Universal columns (UC)

Swipe horizontally to view all dimensions.

Designation Mass (kg/m) h (mm) b (mm) tw (mm) tf (mm) r (mm)
UC 356 × 406 × 1299 1299 600 476 100 140 20
UC 356 × 406 × 1202 1202 580 471 95 130 20
UC 356 × 406 × 1086 1086 569 454 78 125 20
UC 356 × 406 × 990 990 550 448 71.9 115 20
UC 356 × 406 × 900 900 531 442 65.9 106 20
UC 356 × 406 × 818 818 514 437 60.5 97 20
UC 356 × 406 × 744 744 498 432 55.6 88.9 20
UC 356 × 406 × 677 677 483 428 51.2 81.5 20
UC 356 × 406 × 634 634 474.6 424 47.6 77 20
UC 356 × 406 × 592 592 465 421 45 72.3 20
UC 356 × 406 × 551 551 455.6 418.5 42.1 67.5 20
UC 356 × 406 × 509 509 446 416 39.1 62.7 20
UC 356 × 406 × 467 467 436.6 412.2 35.8 58 20
UC 356 × 406 × 393 393 419 407 30.6 49.2 20
UC 356 × 406 × 340 340 406.4 403 26.6 42.9 20
UC 356 × 406 × 287 287 393.6 399 22.6 36.5 20
UC 356 × 406 × 235 235 381 394.8 18.4 30.2 20
UC 356 × 368 × 202 202 374.6 374.7 16.5 27 20
UC 356 × 368 × 177 177 368.2 372.6 14.4 23.8 20
UC 356 × 368 × 153 153 362 370.5 12.3 20.7 20
UC 356 × 368 × 129 129 355.6 368.6 10.4 17.5 20
UC 305 × 305 × 283 283 365.3 322.2 26.8 44.1 20
UC 305 × 305 × 240 240 352.5 318.4 23 37.7 20
UC 305 × 305 × 198 198 339.9 314.5 19.1 31.4 20
UC 305 × 305 × 158 158 327.1 311.2 15.8 25 20
UC 305 × 305 × 137 137 320.5 309.2 13.8 21.7 20
UC 305 × 305 × 118 118 314.5 307.4 12 18.7 20
UC 305 × 305 × 97 96.9 307.9 305.3 9.9 15.4 20
UC 254 × 254 × 167 167 289.1 265.2 19.2 31.7 13
UC 254 × 254 × 132 132 276.3 261.3 15.3 25.3 13
UC 254 × 254 × 107 107 266.7 258.8 12.8 20.5 13
UC 254 × 254 × 89 88.9 260.3 256.3 10.3 17.3 13
UC 254 × 254 × 73 73.1 254.1 254.6 8.6 14.2 13
UC 203 × 203 × 86 86.1 222.2 209.1 12.7 20.5 10
UC 203 × 203 × 71 71 215.8 206.4 10 17.3 10
UC 203 × 203 × 60 60 209.6 205.8 9.4 14.2 10
UC 203 × 203 × 52 52 206.2 204.3 7.9 12.5 10
UC 203 × 203 × 46 46.1 203.2 203.6 7.2 11 10
UC 152 × 152 × 51 51 170.2 157.4 11 15.7 8
UC 152 × 152 × 44 44 166 155.9 9.5 13.6 8
UC 152 × 152 × 37 37 161.8 154.4 8 11.5 8
UC 152 × 152 × 30 30 157.6 152.9 6.5 9.4 8
UC 152 × 152 × 23 23 152.4 152.2 5.8 6.8 8

HE M (HEM) can still be quoted when it is named on the enquiry and is in the mill programme; a complete HEM table is not reproduced here. Chinese HW/HM/HN sizes belong to GB/T 11263. American W-shapes belong to ASTM A36 or ASTM A572 practice, not to these HEA, HEB, IPE, UB or UC rows.

S235JR Chemical Composition (EN 10025-2 Ladle Analysis)

The figures below are ladle-analysis maxima for S235JR long products in EN 10025-2:2019. They are limits, not typical heat results. Do not mix them with unofficial tables that borrow plate phosphorus figures or that give S235JR a silicon maximum it does not generally have.

Element Ladle analysis, max (mass %) Notes for S235JR long products
C, t ≤ 16 mm 0.17 —
C, 16 mm < t ≤ 40 mm 0.17 —
C, t > 40 mm 0.20 For nominal thickness greater than 100 mm, carbon is subject to agreement.
Si No general maximum A dash in the source table. By agreement, silicon may be set at 0.14–0.25% and phosphorus at ≤0.035% for hot-dip galvanizing category B.
Mn 1.40 —
P 0.040 See the galvanizing agreement above. Do not paste a flat-product 0.035% default onto a beam order unless that is what was agreed.
S 0.040 —
N 0.012 The nitrogen maximum does not apply if total aluminium is at least 0.020%, or if sufficient other nitrogen-binding elements are present and reported.
Cu 0.55 —
Other added elements As reported If other elements are added, they shall be mentioned on the inspection document.

S235JR Carbon Equivalent

The carbon equivalent is calculated from the ladle analysis by CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Cu + Ni)/15. The EN 10025-2:2019 maxima for S235JR long products are:

Nominal thickness (mm) Maximum CEV (ladle analysis, %)
t ≤ 30 0.35
30 < t ≤ 40 0.35
40 < t ≤ 140 0.38

The third band applies to nominal thicknesses greater than 40 mm and not more than 140 mm. For thicknesses above 140 mm, a carbon-equivalent limit is not tabulated here and must be agreed and verified on the order; no value is invented for that range. Clause 7.2.5 of EN 10025-2:2019 addresses special conditions for S275 and S355; those conditions are not applied to S235JR on this page.

S235JR Mechanical Properties: Yield, Tensile and +20 °C Impact

Tensile properties of S235JR are thickness-dependent. The values below are from EN 10025-2:2019 for long products, with elongation based on L0 = 5.65√S0. For sections with nominal thickness greater than 100 mm, the mechanical values shall be agreed and verified on the order; the 100–150 mm row is the published long-product band and is not an invented extension. No mechanical limits beyond 150 mm are given here. Plate elongation and sampling are covered on S235JR steel plate, not by this table.

Nominal thickness t (mm) Minimum yield ReH (MPa) Tensile strength Rm (MPa) Minimum elongation A (%)
t ≤ 16 235 360–510 26
16 < t ≤ 40 225 360–510 26
40 < t ≤ 63 215 360–510 25
63 < t ≤ 80 215 360–510 24
80 < t ≤ 100 215 360–510 24
100 < t ≤ 150 195 350–500 22

Quality JR requires a Charpy V-notch absorbed energy of 27 J at +20 °C. For long products the test is normally longitudinal unless the order specifies otherwise. If the project needs 27 J at 0 °C or at −20 °C, the grade to nominate is S235J0 or S235J2, not S235JR.

Apply the band that matches the governing thickness, usually the flange. An HE 300 B flange is 19 mm, so the minimum yield is 225 MPa, not 235 MPa.

Delivery Conditions, Inspection and Identification

S235JR sections are commonly supplied in the as-rolled condition. The inspection document should show EN 10025-2 and its edition, the grade S235JR (1.0038), the EN 10365 size designation, the EN 10034 edition used for tolerances, the delivery condition, the heat number, ladle analysis, the carbon equivalent, and the tensile and +20 °C impact results.

An EN 10204 type 3.1 document is the usual export request; type 3.2 or nominated third-party attendance can be added when the specification requires it. Identification on the product follows the mill’s marking practice and the ordered standards.

Length is not fixed by the size table. Mills commonly roll these sections in fixed lengths in the region of 6–15 m, or in other agreed lengths, according to the rolling programme and the order.

Weldability and Surface Condition of S235JR H-Beams

S235JR is a weldable non-alloy structural steel when thickness, joint design and hydrogen control are taken into account. The CEV table above is the starting point; the certificate values and a procedure suited to the thickness are the practical controls. This page does not prescribe a procedure or a preheat chart.

The as-rolled surface is mill scale. A blast class, a paint system, or a hot-dip galvanizing chemistry is an order option. If galvanizing is planned, the optional Category B silicon and phosphorus limits in the material table, and the processor’s coating specification, should be reviewed before production. Surface quality for sections is commonly specified to EN 10163-3; the class belongs in the enquiry when it matters.

Cutting to length, weld-end preparation, forming or coating can be reviewed when the specification is sent with the enquiry. They are not assumed for every size.

EN 10034 Shape Tolerances and Theoretical Mass

Dimensional and mass tolerances for these I and H sections are those of EN 10034, not of EN 10025-2. This article does not reproduce the millimetre tolerance tables; acceptance is against the edition named on the order.

The size tables above are nominal reference dimensions. A delivered HE 200 A will measure close to 190 × 200 × 6.5 × 10 mm within those tolerances, not as a set of exact advertised millimetres. Out-of-square and web off-centre matter for end-plate connections.

The kg/m column is a theoretical catalogue mass. Weighed mass may sit above or below that figure and still be within tolerance. Settlement should follow the contract — theoretical mass or weighed mass — not an informal mix of those bases.

Applications and Service Limits

S235JR H-beams are used where a 235 MPa yield class and a +20 °C impact quality are accepted:

  • Building frames, workshops, platforms and general structural fabrication.
  • Members that the specification actually names as S235JR, rather than S275JR or S355JR.
  • Export packages that compare the grade with Q235B or ASTM A36, provided each line keeps its own standard and shape system.

It is not specified here for pressure equipment, for nuclear safety-related components, or for structures whose specification requires a lower impact-test temperature or a 355 MPa grade. Durability comes from the coating or fire-protection system, not from the grade name.

S235JR Compared with S355JR, Q235B and A36

S235JR and S355JR share the HEA, HEB and IPE shape system, but they are different yield classes, with different chemistry and carbon-equivalent tables. An enquiry that says only “European H-beam” is incomplete. S235J0 and S235J2 keep the 235 MPa class but move the 27 J impact test to 0 °C and −20 °C, and they use tighter phosphorus and sulphur.

Q235B under GB/T 700, rolled as HW/HM/HN to GB/T 11263, is a near-equivalent in yield class, with a 27 J impact requirement at +20 °C and a different chemistry table. ASTM A36 wide-flange beams are a 36 ksi [250 MPa] grade on W-shapes to ASTM A6. Dual certification is possible only when the delivered piece meets every requirement of each named standard.

Near-Equivalents: Not Automatic Substitutes

The comparisons below are for orientation. They are not a licence to substitute one grade for another on a contract or an inspection certificate.

Grade / designation Standard Relationship to S235JR H-beam Caution
S235J0 / S235J2 EN 10025-2 Same 235 MPa yield class. J0 is tested at 0 °C and J2 at −20 °C, both at 27 J. J0 and J2 also use tighter phosphorus and sulphur. They are not interchangeable with JR on a +20 °C specification.
Q235B GB/T 700; dimensions GB/T 11263 A 235 MPa Chinese carbon steel with a 27 J impact requirement at +20 °C. Different chemistry table and the HW/HM/HN shape system, not HEA/HEB/IPE.
ASTM A36 ASTM A36/A36M; dimensions ASTM A6 A general structural carbon steel, often compared in export enquiries. Yield class is 36 ksi [250 MPa], not 235 MPa, and the shape system is W, not HEA/HEB/IPE.
SS400 JIS G 3101; dimensions often JIS G 3192 A general-structural carbon steel used on Japanese and Taiwanese projects. SS400 has its own tensile window and no JR/J0/J2 impact ladder.

Sister beam pages in this series (S275JR, Q235B, A36, SS400) will be linked here once they are published. Until then, use the live category and plate links above, and the published S355JR H-beam page for the 355 MPa European comparison.

Sourcing S235JR H-Beams from SHH STEEL

SHH STEEL supplies S235JR H-beams as an export trading house, coordinating mill production and project procurement. The useful part of that model is to align the material edition (EN 10025-2), the quality letters (JR, not an unspoken J0 or J2), the shape standard (EN 10365) and tolerance standard (EN 10034), the exact HEA, HEB or IPE designation, and the inspection document before a rolling programme is committed.

Sections can be sourced from mills that SHH STEEL buys from, including Masteel, Rizhao Steel, Laiwu (Shandong Steel Laiwu) and Tung Ho Steel, among others when the programme matches the order. Those mills do not each roll every HEA, HEB or IPE size in S235JR. Mid-range sizes are the usual core; the heaviest HE rows and uncommon IPE variants are confirmed per line. Mixed procurement can be used when a take-off spans more than one rolling programme.

The same enquiry can also cover Chinese, American or Japanese designations, provided each line states its material standard, shape standard and size. If cutting, weld-end preparation, forming or a coating system is required, include that specification for review. Export packing and container loading can be arranged to the packing list agreed for the shipment.

S235JR H-Beam FAQs

Can I replace an HEA or HEB with a W-shape or an HW of the same depth?
No. HEA, HEB and IPE follow EN 10365 and EN 10034. W-shapes follow ASTM A6, and HW/HM/HN follow GB/T 11263. HE 300 A is 290 mm deep and is not a W12 or an HW 300×300. Select the section from the standard named on the drawing, or obtain a formal design change.
Is S235 the same as S235JR?
S235 is the yield class; JR, J0 and J2 are qualities. JR is tested at +20 °C, J0 at 0 °C and J2 at −20 °C, all at 27 J, and J0/J2 have tighter phosphorus and sulphur. An order that says only “S235 H-beam” is incomplete.
Does S235JR have a silicon maximum?
There is no general silicon maximum in the S235JR long-product table used here. By agreement, silicon may be set at 0.14–0.25% and phosphorus at not more than 0.035% when hot-dip galvanizing category B is required. That agreement should appear on the order.
Is S235JR the same as Q235B or ASTM A36?
They are near-equivalents in a general-structural carbon class, not automatic substitutes. Q235B is a GB/T 700 grade, usually supplied as HW/HM/HN. A36 is a 36 ksi [250 MPa] ASTM grade, usually supplied as W-shapes. Chemistry, tests and dimensions all have to be met if dual certification is requested.
Which standards should appear on the inspection document?
At least EN 10025-2 and its edition, the grade S235JR (1.0038), the EN 10365 designation, the EN 10034 edition used for tolerances, the delivery condition, ladle analysis, the carbon equivalent, tensile results by thickness, and the +20 °C impact result.

Request a Quotation for EN 10025-2 S235JR H-Beam

EN 10025-2 S235JR H-beam is a non-alloy structural section with 235 MPa minimum yield up to 16 mm and a 27 J impact requirement at +20 °C. Nominate the HEA, HEB or IPE size to EN 10365, the tolerances to EN 10034, and the material to EN 10025-2 (or the edition on the order). The tables are reference dimensions, not a rolling list. Send the size list, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X