CCS Grade A shipbuilding steel plate to China Classification Society (CCS) rules, stacked hull plates

CCS Grade A Shipbuilding Steel Plate

CCS Grade A (CCS A) normal-strength hull structural steel plate, yield 235 N/mm² min., Charpy at +20 °C where required, stamped CCS Grade A / CCS A with China Classification Society–endorsed certificates. SHH STEEL supplies CCS Grade A / CCS A shipbuilding plate from stock in China, with cutting, multi-class certification and third-party inspection.
Keywords
CCS Grade A steel plate, CCS A shipbuilding steel plate, CCS Grade A marine plate, CCS A hull steel, China Classification Society Grade A plate, normal strength hull structural steel, GB 712 Grade A
Equivalent Grades:
ASTM A131 Grade A; ABS A; DNV NV A; LR Grade A; BV Grade A; NK KA; KR RA; RINA Grade A; GB 712 Grade A
Share:
Overview
Specification
Chemical Composition
Mechanical Properties
Impact Test and Condition of Supply
Thickness Tolerance
Stock
Equivalent Grades
Grade Selection
Applications and Fabrication
Testing and Inspection
Specification Mistakes
Buyer Concerns
How to Order
FAQ
Conclusion

CCS Grade A / CCS A shipbuilding steel plate — overview

Technical Reviewer: Jack | SHH STEEL Material Solutions Department · Updated: 2026-10-27

CCS Grade A, commercially written CCS A on mill certificates and plate markings, is the ordinary-strength (normal-strength) hull structural steel under China Classification Society (CCS) Rules for Materials that implement IACS UR W11 for normal and higher strength hull steels. It is often ordered alongside GB 712 Grade A plate from the same Chinese mills, but GB 712 is a product standard — CCS class approval and the CCS A stamp are what a CCS-classed hull needs. Minimum yield is 235 N/mm², tensile 400–520 N/mm² and 22 % minimum elongation (A5). Up to 50 mm thickness Charpy is generally not required; above 50 mm the impact route follows the UR W11 / CCS Materials supply table. Commercial enquiries use CCS Grade A, CCS A shipbuilding steel plate or CCS A marine plate.

Equivalent grades: CCS Grade A ≈ ASTM A131 Grade A ≈ ABS A ≈ DNV NV A ≈ LR Grade A ≈ BV Grade A ≈ NK KA ≈ KR RA ≈ RINA Grade A ≈ GB 712 Grade A (all class-approved, stamped by the issuing society).

Because CCS A needs no Charpy up to 50 mm in the usual supply routes, it is the economical choice for general hull plating on CCS-classed newbuildings and repairs. Where the drawing calls for CCS Grade B, D or E, Grade A cannot be substituted downward. CCS Grade A / CCS Grade A / CCS Grade A raise toughness without raising yield.

Plates that pass mill tests under CCS survey are die-stamped or stencilled CCS Grade A or CCS A (plus Z or U where through-thickness or ultrasonic requirements apply) and are supplied with a mill certificate the CCS Surveyor endorses. SHH STEEL supplies CCS A plate from Chinese mills that hold CCS works approval for the grade, from stock in common sizes or from a mill rolling cycle, with CCS survey arranged at the mill.

CCS CCS A plate: specification summary

ItemCCS Grade A / CCS A data
Rule basisChina Classification Society Rules for Materials (hull structural steel); IACS UR W11 normal-strength Grade A (CCS Materials paragraph cross-refs UNCERTAIN without local CCS PDF)
Related product standardGB 712 Grade A — chemistry/tensile intent aligned; GB 712 alone is not CCS class approval
Strength levelnormal (ordinary) strength, yield strength ReH 235 N/mm² min.
Plate thickness primarily coveredup to 100 mm under IACS UR W11 scope for plates; greater thickness by special consideration under CCS Materials rules (see UNCERTAIN)
Steelmakingbasic oxygen, electric furnace or open-hearth, or other process specially approved by CCS
Deoxidationany except rimmed ≤50 mm; killed >50 mm
Fine grainnot mandatory for all thicknesses (see UR W11 Table 1 / supply table)
Condition of supplyper UR W11 / CCS Materials Table for Grade A (AR/CR/N/TM by thickness — confirm on PO)
Impact testgenerally not required ≤50 mm; >50 mm at +20 °C unless fine-grain N (TM at Society discretion)
MarkingCCS Grade A / CCS A; plus Z / U / TM where ordered and qualified
Thickness toleranceIACS UR W13 as adopted by CCS (minus tolerance commonly 0.3 mm class — confirm on PO; see UNCERTAIN)
Certificatemill certificate endorsed by the CCS Surveyor; EN 10204 3.1 / 3.2 on request

Size range. CCS A is rolled on wide plate mills in China from about 5 mm to 100 mm and more, widths 1500–3500 mm and lengths up to about 18 m depending on mill; 6–25 mm plate in 1800–2500 mm width is the bulk of the market. Plates under about 6 mm are often cut from CCS-approved hot-rolled coil, which needs separate approval of the coil process. Ask for confirmation for plates over 100 mm or wider than 3200 mm.

CCS Grade A / CCS A chemical composition (heat and product analysis)

ElementHeat (ladle) analysis, %Product (check) analysis, %Note
C0.21 max.numeric tolerance not tabulated in CCS Rules for Materials and Welding – agree on order / mill certificateplates; sections may differ where notes allow
Mn2.5 × C min.numeric tolerance not tabulated in CCS Rules for Materials and Welding – agree on order / mill certificateC-linked minimum (2.5 × C)
Si0.50 max.numeric tolerance not tabulated in CCS Rules for Materials and Welding – agree on order / mill certificate
P0.035 max.numeric tolerance not tabulated in CCS Rules for Materials and Welding – agree on order / mill certificate
S0.035 max.numeric tolerance not tabulated in CCS Rules for Materials and Welding – agree on order / mill certificatelower S may be agreed for cold-flanging quality
Other intentionally added elementsto be determined and reportednot tabulated in CCS Rules for Materials and Welding – agree product limits on orderIACS UR W11 Table 1 notes; CCS applies via CCS Rules for Materials
C + Mn/60.40 max.not applicable (calculated from heat analysis)carbon + 1/6 manganese cap

Product (check) analysis column: CCS Rules for Materials and Welding specify heat (ladle) limits; no numeric product-analysis tolerance is tabulated in the rule text reviewed, so product (check) limits are agreed on the order or taken from the approved mill specification and certificate.

Source: IACS UR W11 Table 1 (ladle samples) for normal-strength Grade A — the chemistry China Classification Society applies to CCS A hull plate under CCS Rules for Materials. The same ladle limits appear in GB 712 for Grade A, which is why mills often dual-produce GB 712 and CCS class plate from one heat; the Surveyor endorsement is what turns the product into class steel. Heat (ladle) analysis is determined by the mill on each heat and must meet Table 1. Product (check) analysis on the finished plate is not given numeric tolerances in UR W11 itself; when a purchaser or Surveyor requires product analysis on the certificate, ask at enquiry and record the agreed tolerances — do not invent numbers.

Grade A uses the C-linked manganese rule (Mn ≥ 2.5 × C) and allows the widest Si cap (0.50 %). It is the only ordinary-strength grade that may be supplied without fine-grain practice in the thinner bands. In practice Chinese mills supply aluminium-killed CCS A; treat typical ladle figures as indicative only and check the actual mill certificate.

CCS CCS A tensile properties

PropertyRequirement (IACS UR W11 Table 6)
Tensile strength Rm400–520 N/mm²
Yield strength ReH235 N/mm² min. (or Rp0.2 where ReH cannot be determined)
Elongation A522 % min. (5.65 √S0)
Impact test temperature+20 °C

On the 200 mm gauge full-thickness flat specimen (25 mm width), minimum elongation depends on thickness:

Thickness (mm)≤5>5–10>10–15>15–20>20–25>25–30>30–40>40–50
Elongation min. %1416171819202122

All four normal-strength grades share these tensile values. For each batch, one tensile test is taken from one piece (extra tests when finished weight exceeds 50 t, and for every 10 mm variation in thickness from the same cast), unless otherwise agreed by CCS.

CCS CCS A: Charpy at +20 °C and supply condition

generally not required ≤50 mm; >50 mm at +20 °C unless fine-grain N (TM at Society discretion). Deoxidation: any except rimmed ≤50 mm; killed >50 mm. Average energies at +20 °C (full-size specimens, long / trans) per IACS UR W11 Table 6:

ThicknessLongitudinal (J min.)Transverse (J min.)
t ≤ 502720
50 < t ≤ 703424
70 < t ≤ 1004127

One individual value may fall below the average if it is at least 70 % of it. Generally only longitudinal specimens are prepared unless the purchaser or CCS asks for transverse. The test frequency and permitted delivery condition (AR, CR, N or TM) follow the UR W11 / CCS Materials supply-condition table for Grade A, so write the condition into the PO. Beyond 100 mm thickness is special consideration with CCS (see UNCERTAIN).

Thickness tolerance and surface condition

China Classification Society applies the thickness tolerances of IACS UR W13 (Thickness tolerances of steel plates and wide flats) unless the purchase order states otherwise. In practice class-approved hull plate is ordered to the class minus-tolerance band commonly associated with UR W13 (often 0.3 mm minus — confirm the exact class and plus tolerance on the PO; see UNCERTAIN). Plus tolerance, flatness, width and length follow the agreed national or international standard (for example ASTM A6, EN 10029 or GB/T 709) unless specified otherwise.

Surface quality follows a recognised standard such as EN 10163 parts 1–2 or the equivalent GB surface standard accepted by CCS. Surface defects may be ground within UR W11 limits; grinding areas are checked so remaining thickness stays within the allowed minus tolerance. If you plan to shot-blast and prime at the yard, state any surface class on receipt in the order.

CCS CCS A plate stock in China

Thickness (mm)Width (mm)Length (mm)ConditionApprox. quantityLocation
61800 / 20006000 / 8000AR / CR / N / TM100+ tChina
81800 / 20008000 / 12000AR / CR / N / TM200+ tChina
102000 / 22008000 / 12000AR / CR / N / TM200+ tChina
122000 / 2200 / 250012000AR / CR / N / TM200+ tChina
142000 / 220012000AR / CR / N / TM100+ tChina
162000 / 250012000AR / CR / N / TM200+ tChina
202000 / 250012000AR / CR / N / TM100+ tChina
252200 / 250012000AR / CR / N / TM100+ tChina
30220010000 / 12000AR / CR / N / TM100+ tChina
40220010000AR / CR / N / TM50+ tChina
5022008000 / 10000AR / CR / N / TM50+ tChina

Quantities are approximate and change daily (indicative — confirm before booking); all stock plates carry CCS A marking and CCS-endorsed mill certificates when sold as CCS class plate. Sizes outside the table (for example 3000 mm width, 60–100 mm thickness, or fixed lengths for a cutting plan) are produced in the next mill rolling cycle, typically 3–6 weeks including CCS survey. Send your size list and we will reply with what is in stock and what must be rolled.

Packing. Plates are bundled by size with steel strapping, marked with heat number, grade and CCS stamp, and shipped in containers (up to about 11.8 m) or break bulk for longer plates.

CCS Grade A equivalents in other rules and standards

Standard / societyDesignationComment
CCS (China Classification Society)CCS Grade A / CCS Athis page; stamped under CCS survey
GB 712GB 712 Grade AChinese ship steel product standard; not class approval by itself
ASTM A131/A131MASTM A131/A131M Grade Asame base chemistry and tensile band; A131 is a product standard, not class approval
ABSABS AIACS UR W11 ordinary-strength; live product page
DNVDNV NV AIACS UR W11; live product page
LRLR Grade A / LR/AIACS UR W11; live product page
BVBV Grade AIACS UR W11; live product page
NK (ClassNK)NK KAClassNK designation KA
KRKR RAKR designation RA
RINARINA Grade AIACS UR W11; category link only
ASTM A36ASTM A36similar strength band but not a hull steel; no class marking
EN 10025-2EN 10025-2 S235JR / S235J0 / S235J2structural; J0 has 0 °C test, J2 −20 °C
JIS G3106JIS G3106 SM400A / SM400Bwelded-structure steel; SM400B adds a 0 °C test

These are comparisons, not substitutions. A CCS-classed hull needs plate made by a mill approved by China Classification Society for this grade and certified under CCS survey. Dual or multi-class certification (for example CCS + ABS, CCS + DNV, CCS + LR or CCS + BV) can be arranged at the mill when the heat is surveyed by both societies. Do not treat a GB 712 certificate alone as a substitute for the CCS A stamp.

CCS CCS A vs Grade A/B/D/E and vs structural steels

All four normal-strength grades share the same 235 N/mm² yield and 400–520 N/mm² tensile range; they differ in deoxidation and toughness. Compared with CCS Grade B, Grade A needs no CVN up to 50 mm; Grade B adds 0 °C where the supply table requires it. Grade D (−20 °C) and Grade E (−40 °C) go further for colder service. The hull steel grade for each strake is set by the classification rules according to structural member category and thickness, so check the approved drawing first. Sheer strakes, bilge strakes, deck stringers and ice-belt plating usually call for B, D, E or higher-strength plates under CCS.

Compared with land structural steels, CCS A is close in strength to ASTM A36, ASTM A283 Grade C and S275JR class steels but differs in class thickness tolerance practice, the C + Mn/6 ≤ 0.40 cap, and above all the CCS survey and CCS A stamp. For a CCS-classed vessel only CCS-certified plate is accepted.

When CCS CCS A is the right choice: typical uses are general hull plating and members where the material class does not require an impact test up to 50 mm — side shell, bottom shell, deck plating and secondary members on CCS-classed newbuildings and repairs. The Charpy temperature (+20 °C) is fixed by the letter A, and the strength by the normal-strength level (ReH 235 N/mm²). Pick the strength from the scantling calculation and the letter from the material class and design temperature on the approved drawing. Swapping to a different letter or strength needs class approval of the drawing change, not just a new purchase order.

Applications, cutting and welding of CCS CCS A

Typical uses: general side and bottom shell, strength deck plating where no CVN is required, pontoons and barges, inland and coastal vessels, and ship-repair replacement steel on CCS-classed tonnage. Offshore and port structures also use ordinary-strength grades for secondary steel; see offshore platform steel plates for primary structure grades.

Cutting: oxy-fuel, plasma and laser cutting all work without preheat in normal thicknesses. Welding: with C + Mn/6 at or below 0.40 %, CCS A is welded with ordinary-strength consumables approved for the grade and +20 °C toughness level required by the shipyard’s CCS-approved WPS; preheat is generally unnecessary below about 25–30 mm except in cold or humid conditions — follow your approved welding procedure, not a generic number from a catalogue. Forming: plates intended for cold flanging should be ordered with the flanging quality agreed on the PO.

Processing notes for CCS A: cold forming and flanging of normal-strength plate are routine. Keep the cut edges of plate thicker than 50 mm free of notches, because thick plate of this grade is controlled more tightly for deoxidation (any except rimmed ≤50 mm; killed >50 mm).

Certificates, CCS survey and third-party inspection

Every plate is tested and marked at the mill under China Classification Society survey; the mill certificate lists heat number, ladle chemistry (elements required by UR W11 Table 1, plus intentionally added elements), tensile results, impact results at +20 °C where required, condition of supply and plate numbers, and is endorsed by the attending Surveyor. On request we add EN 10204 3.2 certificates with third-party witness by TÜV, SGS, LR or another agency, ultrasonic testing (U mark) or through-thickness testing (Z mark), and multi-class certification with other major class societies (ABS, DNV, LR, BV, NK, KR, RINA).

On receipt, check: CCS Grade A / CCS A stamp and heat number on each plate match the certificate; the certificate shows CCS endorsement, not just a mill or GB 712 stamp; thickness at several points meets the ordered UR W13 / PO tolerance; impact results agree with the table below for the delivered thickness.

Charpy acceptance for CCS A by thickness (from IACS UR W11 Table 6; actual results as per standard and mill certificate):

Thickness t (mm)Test temperatureAverage energy, longitudinal (J min.)Average energy, transverse (J min.)
t ≤ 50+20 °C2720
50 < t ≤ 70+20 °C3424
70 < t ≤ 100+20 °C4127

On receipt, check that the test temperature is +20 °C and that the energy matches the band for the delivered thickness. Also check that the plate number on the stamp matches the certificate line, and that the CCS Surveyor endorsement is present. If UT was ordered (e.g. EN 10160 or ASTM A578 level), check the UT report as well. If the PO asked for 3.2, the inspector’s report must name the witnessed tests and plate numbers.

Common mistakes when ordering CCS Grade A / CCS A

  • Ordering “CCS A” or “Grade A” without requiring China Classification Society certification (CCS Grade A / CCS A stamp + Surveyor-endorsed certificate)
  • Accepting GB 712 or ASTM A131 certificates alone for a CCS-classed hull
  • Ignoring C + Mn/6 ≤ 0.40 on the ladle analysis
  • Substituting CCS Grade A where the drawing requires Grade B, D or E
  • Coil-cut plate without CCS coil-process approval
  • Confusing Grade A with higher-strength CCS A32 / AH32

Each of these is avoided by writing the requirement into the purchase order and checking it on the certificate before the plates are cut.

Sourcing CCS CCS A plate: buyer concerns and SHH STEEL solutions

ConcernHow SHH STEEL handles it
Fake or re-stamped class plateplates from CCS-approved mills only; certificate and CCS A stamp traceable to the heat; third-party witness and EN 10204 3.2 on request
Unsafe deposit or payment riskT/T or L/C payment; inspection before balance payment
Small quantities across many sizesmixed thicknesses and grades (CCS A, CCS Grade A/B/D/E, A36 / AH36, etc.) combined in one container or shipment
Slow deliverydedicated staff follow each order with weekly production and shipping updates and photos
Cutting and preparationown workshop for cutting to size, bevelling, drilling and machining before shipment

How to order CCS CCS A plate

State the grade and rule (CCS Grade A / CCS A, China Classification Society Rules for Materials – rolled steel for hull), whether multi-class certification is needed, thickness, width, length and quantity per size, condition of supply, any Z or U requirement, surface or primer requirements, certificate type (mill certificate with CCS endorsement, EN 10204 3.2 with third-party witness), packing and destination port. Send the list to SHH STEEL for price, available stock and lead time.

Sample PO line: “Steel plate to China Classification Society Rules for Materials, Grade A (CCS A), delivery condition [AR/CR/N/TM], 20 × 2500 × 12000 mm, 30 pcs, marked CCS Grade A / CCS A, certificate endorsed by CCS Surveyor, EN 10204 3.2 [if required], UT [if required], CIF [port].” Each bracketed item changes price, lead time and which mills can supply, so fix them at enquiry stage.

FAQ

What sizes and minimum order quantity can you supply for CCS Grade A / CCS A plate?
Under IACS UR W11 the primary plate scope is up to 100 mm thick; thicker plate is a special-consideration item with China Classification Society. Common CCS A hull plate runs 6–50 mm thick, 1500–3000 mm wide and 6000–12000 mm long; thinner coil-cut sizes and wider plates are mill-roll items. Stock plate has no fixed minimum — one plate can be supplied, cut to size if you like. A mill rolling for a special width or length usually needs a minimum quantity per size, which depends on the mill and the slot, so we confirm it with each quote. Mixed sizes of CCS A with other CCS ordinary- or higher-strength grades in one shipment are routine for repair yards and small newbuildings.
How is CCS Grade A / CCS A certified, and can you arrange EN 10204 3.2 or dual-class with ABS/DNV/LR/BV?
Every plate is made by a CCS-approved mill under China Classification Society survey. It is die-stamped or stencilled CCS Grade A / CCS A with the heat or plate number, and the mill test certificate is endorsed by the CCS Surveyor. The certificate gives the ladle chemistry (UR W11 Table 1 elements), the tensile results (ReH ≥ 235 N/mm², Rm 400–520 N/mm², A5 ≥ 22 %), the Charpy results at +20 °C where required, the delivery condition and the plate identity. A GB 712 Grade A certificate alone is not CCS class approval. If your contract asks for EN 10204 3.2, we arrange it before rolling. Dual or multi-class stamping (CCS + ABS, DNV, LR or BV) must be booked before testing so both Surveyors attend the same heat. 3.2 cannot be added after the plates have been tested, so please state it on the enquiry.
What is the impact test temperature and energy for CCS Grade A / CCS A, and when is Charpy required?
CCS A is tested at +20 °C (generally not required ≤50 mm; >50 mm at +20 °C unless fine-grain N (TM at Society discretion)). The average energies (longitudinal/transverse, J min.) depend on thickness: ≤50 mm 27/20; 50–70 mm 34/24; 70–100 mm 41/27. Deoxidation: any except rimmed ≤50 mm; killed >50 mm. The test frequency per batch or per plate follows the delivery condition in the UR W11 / CCS Materials supply table, so the PO should state the condition (AR, CR, N or TM). Final results are as per standard and mill certificate. Beyond 100 mm agree special consideration with CCS.
What welding and preheat guidance applies to CCS CCS A?
CCS A is a C–Mn hull steel with C 0.21 max. and C + Mn/6 ≤ 0.40, and is generally easy to weld. China Classification Society does not publish a single preheat value for the plate grade itself. Preheat, interpass temperature, heat input and consumables come from the shipyard’s CCS-approved welding procedure (WPS/PQR), using consumables approved for the +20 °C toughness level needed. Thick or highly restrained joints may need preheat under that approved procedure. Ask us for the actual ladle analysis on the mill certificate early so your welding engineer can check carbon equivalent. We do not give fixed preheat numbers for the grade, because the approved procedure always governs.
What is the delivery time for CCS CCS A plate from stock or mill rolling?
Stock sizes of CCS A can usually be cut, inspected and loaded in about 7–15 days. Mill-rolled orders typically take about 3–6 weeks plus inspection, depending on thickness, delivery condition and the mill schedule. These are commercial estimates, confirmed with each quote — not contractual lead times until the PI is accepted. If 3.2 witness or multi-class survey is required, we book the inspector when we place the mill order so testing is not delayed. A dedicated coordinator sends weekly progress photos (rolling, marking, testing, packing, loading) until the bill of lading is issued.
Which payment terms do you accept for CCS Grade A, and how is the deposit protected?
We accept T/T or L/C at sight. With T/T, the usual terms are a 30 % deposit and the balance against the documents or after inspection. You or your inspector can check the CCS A stamping, the dimensions and the Surveyor-endorsed certificate before you pay the balance, so the plate is verified before most of the money moves. With L/C, payment is tied to the presented documents (commercial invoice, packing list, B/L, mill certificate, and the 3.2 or class certificate if you require one). For first orders we can start with a smaller trial lot. The proforma invoice shows the grade (CCS Grade A / CCS A), sizes and certificate type, so the contract and the delivered plate match.
What are the equivalent grades of CCS CCS A among other class societies and GB 712?
CCS Grade A / CCS A is treated as equivalent in strength and chemistry intent to ASTM A131/A131M Grade A, ABS A, DNV NV A (DNV Grade A), LR Grade A, BV Grade A, NK KA, KR RA, RINA Grade A, and GB 712 Grade A. All follow IACS UR W11 for ordinary-/normal-strength hull steel (ReH ≥ 235 N/mm², Rm 400–520 N/mm²). “Equivalent” does not mean interchangeable on paper. Each society accepts only its own stamp and certificate, so CCS-classed construction needs CCS A, not a GB 712 certificate alone. Where a vessel is dual-classed, we can arrange joint survey so one plate carries both stamps (e.g. CCS + ABS, CCS + DNV, CCS + LR, CCS + BV).
Can you cut, bevel or machine CCS CCS A plates, and how are they packed for export?
Yes. In our workshop we can flame, plasma or laser cut CCS A to drawings, bevel weld edges (V, X or K preparation to your angle and land), drill and machine. Every cut piece keeps traceability: we transfer the CCS A marking and heat number before cutting, and the cutting list is tied to the mill certificate. For export, plates are bundled with steel straps and timber spacers, marked with grade, size and heat number, and loaded in containers or as break-bulk. Shot blasting and shop primer are available on request. Loading photos and a packing list come with each shipment. See SHH STEEL for our processing capabilities.

Conclusion

CCS Grade A / CCS A is ordinary-strength hull steel under China Classification Society Rules for Materials and IACS UR W11: 235 N/mm² minimum yield, 400–520 N/mm² tensile, Charpy at +20 °C where required, and class survey with the CCS A stamp. GB 712 Grade A is the related Chinese product standard — not a substitute for CCS class approval. What the rules leave open has to be fixed in the order: CCS (or multi-class) certification, the supply condition and impact testing, whether product analysis is required on the certificate, the thickness-tolerance class, and the certificate type (3.1 vs 3.2).

SHH STEEL supplies CCS A plate rolled by Chinese mills that hold China Classification Society works approval for the grade, so every plate carries the CCS A stamp and a Surveyor-endorsed certificate traceable to its heat. Common thicknesses are available from stock; other sizes are scheduled into the mill rolling cycle with CCS survey arranged at the mill. On request we add EN 10204 3.2 certificates with third-party witness (TÜV, SGS, LR or another agency) and joint certification with ABS, DNV, LR, BV, NK, KR or RINA.

We accept T/T or L/C payment, with inspection before the balance is paid. Small quantities in several sizes, or CCS A mixed with other CCS Grade A/B/D/E or higher-strength grades such as CCS A36 / AH36, can be combined in one container. A dedicated coordinator sends production and shipping updates with photos, and our own workshop cuts to size, bevels, drills and machines plates before shipment so they arrive ready for fabrication.

Request a quotation: send SHH STEEL the grade (CCS A / CCS Grade A), thickness, width, length, quantity per size and destination port, plus any multi-class, Z/U or 3.2 certificate requirement. We reply with price, available stock and lead time.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *



    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *



      X