BV AH40 Shipbuilding Steel Plate
BV AH40 / BV AH40 shipbuilding steel plate — overview
Under Bureau Veritas NR216 Materials rules (IACS UR W11), BV AH40 — stamped BV AH40 — sits in the higher-strength AH family at 0 °C toughness. Strength level 40 means minimum yield 390 N/mm², tensile 510–650 N/mm² and elongation 20 % min. (A5). The letter AH fixes Charpy V-notch testing at 0 °C. In commercial enquiries it is called BV AH40 or BV AH40 shipbuilding steel plate.
Equivalent grades: BV AH40 ≈ ASTM A131 Grade AH40 ≈ ABS AH40 ≈ DNV NV A40 ≈ LR AH40 ≈ CCS A40 / AH40 ≈ NK KA40 ≈ KR RA40 ≈ RINA AH40 ≈ GB 712 Grade AH40 (all class-approved, stamped by the issuing society).
BV AH40 is selected when scantlings need the higher yield of the 40 band and the material class assigns 0 °C toughness. Ordinary-strength BV Grade A–E stay at 235 N/mm² yield and cannot replace AH40 without a drawing change. Within the 40 band, letter choice is toughness: AH 0 °C → DH −20 °C → EH −40 °C → FH −60 °C; within the AH letter, strength steps 32 → 36 → 40 raise yield from 315 to 355 to 390 N/mm².
Plates that pass mill tests under Bureau Veritas survey are die-stamped or stencilled BV AH40 or BV AH40 (plus Z or U where through-thickness or ultrasonic requirements apply) and are supplied with a mill certificate the BV Surveyor endorses. SHH STEEL supplies BV AH40 from Chinese mills that hold Bureau Veritas works approval for the grade, from stock in common sizes or from a mill rolling cycle, with BV survey arranged at the mill.
BV BV AH40 plate: specification summary
| Item | BV BV AH40 / AH40 data |
|---|---|
| Rule basis | Bureau Veritas NR216 Materials; IACS UR W11 higher-strength Grade AH40 (NR216 paragraph cross-refs UNCERTAIN without local BV PDF) |
| Strength level | higher strength 40, yield 390 N/mm² min., tensile 510–650 N/mm² |
| Toughness class | AH → Charpy at 0 °C |
| Plate thickness primarily covered | up to 100 mm under IACS UR W11 scope for plates; greater thickness by special consideration (see UNCERTAIN) |
| Deoxidation | killed, fine grain practice (UR W11) |
| Impact test | Charpy V at 0 °C; frequency and supply condition per UR W11 / NR216 tables |
| Marking | BV AH40 / BV AH40; plus Z / U / TM where ordered and qualified |
| TMCP Ceq (indicative UR W11 / industry practice) | ≤ 0.40 % for t ≤ 50 mm; ≤ 0.42 % for 50 < t ≤ 100 mm (TM steels) — confirm on mill approval / PO |
| Thickness tolerance | IACS UR W13 as adopted by BV (minus tolerance commonly 0.3 mm class — confirm on PO; see UNCERTAIN) |
| Certificate | mill certificate endorsed by the BV Surveyor; EN 10204 3.1 / 3.2 on request |
Size range. Common market thicknesses for AH40 are about 6–80 mm (heavier plates available as per mill approval), widths 1500–3500 mm. Exact maximum thickness for a given delivery condition is as per standard and mill certificate / BV works approval. Ask for confirmation above 100 mm.
BV AH40 / BV AH40 chemical composition (heat and product analysis)
| Element | Heat (ladle) analysis, % | Product (check) analysis, % | Note |
|---|---|---|---|
| C | 0.18 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | AH/DH/EH group |
| Mn | 0.90–1.60 (AH ≤12.5 mm may be 0.70 min.) | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | AH ≤12.5 mm may use 0.70 % Mn min. |
| Si | 0.10–0.50 | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | min. waived if acid-soluble Al ≥ 0.015 % |
| P | 0.035 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | |
| S | 0.035 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | |
| Al (acid soluble) min. | 0.015 min. acid-soluble (or total Al per UR W11 fine-grain practice) | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | grain refining |
| Nb | 0.02–0.05 when used singly | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | when used singly; combined minima in UR W11 |
| V | 0.05–0.10 when used singly | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | when used singly |
| Ti | 0.02 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | need not be reported unless intentionally added |
| Cu | 0.35 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | |
| Cr | 0.20 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | |
| Ni | 0.40 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | |
| Mo | 0.08 max. | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | |
| N | — | numeric tolerance not tabulated in BV NR216 – agree on order / mill certificate | not specified as a max in AH/DH/EH column |
Product (check) analysis column: BV NR216 specify heat (ladle) limits; no numeric product-analysis tolerance is tabulated in the rule text reviewed, so product (check) limits are agreed on the order or taken from the approved mill specification and certificate.
Source: IACS UR W11 higher-strength chemistry tables (ladle samples) — the chemistry Bureau Veritas applies to BV AH40 via NR216. AH/DH/EH share one chemistry column; FH is tighter on C, P, S and adds N control with higher Ni allowance. Toughness is differentiated by impact temperature and supply routes, not by separate C/Mn caps within AH/DH/EH. Product (check) analysis numeric tolerances are not tabulated in UR W11; when required, agree tolerances at enquiry. TMCP steels must also meet the applicable Ceq / Pcm limits on the mill approval — ask for Ceq on the certificate.
BV BV AH40 tensile properties
| Property | Requirement (IACS UR W11) |
|---|---|
| Tensile strength Rm | 510–650 N/mm² |
| Yield strength ReH | 390 N/mm² min. |
| Elongation A5 | 20 % min. |
| Impact test temperature | 0 °C |
Alternative flat-specimen elongations by thickness (indicative UR W11 / industry table for strength 40):
| Thickness (mm) | ≤5 | >5–10 | >10–15 | >15–20 | >20–25 | >25–30 | >30–40 | >40–50 |
|---|---|---|---|---|---|---|---|---|
| Elongation min. % | 12 | 14 | 15 | 16 | 17 | 18 | 19 | 20 |
Same tensile band applies to AH/DH/EH/FH 40; only impact temperature and chemistry group (FH vs AH/DH/EH) change across the letter.
BV BV AH40: Charpy at 0 °C and supply condition
| Thickness | Long. avg. at 0 °C | Trans. avg. at 0 °C |
|---|---|---|
| t ≤ 50 mm | 39 J | 26 J |
| 50 < t ≤ 70 mm | 46 J | 31 J |
| 70 < t ≤ 100 mm | 55 J | 37 J |
Source: IACS UR W11 impact table for higher-strength Grade AH40 (full-size; either direction acceptable unless specified). Energies rise with thickness — a 60 mm plate must meet higher values than a 20 mm plate at the same 0 °C. Condition of supply and impact lot size depend on grain-refining practice and thickness (AR/CR/N/TM/QT as permitted). For TMCP AH40, respect Ceq caps ≈ 0.40 % (t≤50) / 0.42 % (50
Thickness tolerance and surface condition
Bureau Veritas applies IACS UR W13 thickness tolerances unless the PO states otherwise (often 0.3 mm minus class — confirm on PO; see UNCERTAIN). Plus/flatness/width/length per agreed standard (ASTM A6 or EN 10029). Surface quality per EN 10163 or equivalent accepted by BV; state primer/surface class on receipt if needed.
BV BV AH40 plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Condition | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1800 / 2000 | 6000 / 8000 | AR / CR / N / TM | 100+ t | China |
| 8 | 1800 / 2000 | 8000 / 12000 | AR / CR / N / TM | 200+ t | China |
| 10 | 2000 / 2200 | 8000 / 12000 | AR / CR / N / TM | 200+ t | China |
| 12 | 2000 / 2200 / 2500 | 12000 | AR / CR / N / TM | 200+ t | China |
| 14 | 2000 / 2200 | 12000 | AR / CR / N / TM | 100+ t | China |
| 16 | 2000 / 2500 | 12000 | AR / CR / N / TM | 200+ t | China |
| 20 | 2000 / 2500 | 12000 | AR / CR / N / TM | 100+ t | China |
| 25 | 2200 / 2500 | 12000 | AR / CR / N / TM | 100+ t | China |
| 30 | 2200 | 10000 / 12000 | AR / CR / N / TM | 100+ t | China |
| 40 | 2200 | 10000 | AR / CR / N / TM | 50+ t | China |
| 50 | 2200 | 8000 / 10000 | AR / CR / N / TM | 50+ t | China |
Quantities are approximate and change daily (indicative — confirm before booking); all stock plates carry BV AH40 marking and Bureau Veritas–endorsed mill certificates when sold as BV class plate. Sizes outside the table (for example 3000 mm width, 60–100 mm thickness, or fixed lengths for a cutting plan) are produced in the next mill rolling cycle, typically 3–6 weeks including BV survey. Send your size list and we will reply with what is in stock and what must be rolled.
Packing. Plates are bundled by size with steel strapping, marked with heat number, grade and BV stamp, and shipped in containers (up to about 11.8 m) or break bulk for longer plates.
BV BV AH40 equivalents in other rules and standards
| Standard / society | Designation | Comment |
|---|---|---|
| BV (Bureau Veritas) | BV AH40 (BV AH40) | this page; stamped under BV survey |
| ASTM A131/A131M | ASTM A131/A131M Grade AH40 | A131 lists AH–FH 32/36/40; product standard only |
| ABS | ABS AH40 | IACS UR W11 higher-strength; live product page |
| DNV | DNV NV A40 | IACS UR W11; live product page |
| LR | LR AH40 / LR/AH40 | IACS UR W11; live product page |
| CCS | CCS AH40 | IACS UR W11; category link only |
| NK (ClassNK) | NK KA40 | ClassNK KA40 |
| KR | KR RA40 | KR RA40 |
| RINA | RINA Grade AH40 | confirm exact designation per RINA rules |
| GB 712 | GB 712 Grade AH40 | not class approval by itself |
| Structural (indicative) | EN 10025-2 S355JR / S355J2 | land structural; no class marking |
These are comparisons, not substitutions. Multi-class stamps (BV + ABS / DNV / LR) require joint survey before rolling.
BV BV AH40 vs other BV hull grades
Pick AH40 when the drawing specifies higher-strength grade AH40 (or the society equivalent). Do not substitute ordinary Grade A/B unless the designer recalculates scantlings — yield differs (390 vs 235). Within the 40 band, letter choice is toughness: AH 0 °C → DH −20 °C → EH −40 °C → FH −60 °C. Within the AH letter, strength steps 32 → 36 → 40 raise yield from 315 to 355 to 390 N/mm².
For yields above 390 N/mm² Bureau Veritas / IACS move to extra-high strength (UR W16 naming — BV uses A420…F690 without H, not AH420).
When BV BV AH40 is the right choice: typical uses are higher-strength hull girder plating (deck, bottom, side shell) of bulk carriers, tankers and container ships in normal service where 0 °C toughness suffices. The Charpy temperature (0 °C) is fixed by the letter, and the strength by the number (ReH 390 N/mm²). Pick the strength from the scantling calculation and the letter from the material class and design temperature on the approved drawing.
Applications, cutting and welding of BV BV AH40
Typical uses: higher-strength hull girder plating (deck, bottom, side shell) of bulk carriers, tankers and container ships in normal service where 0 °C toughness suffices; weight-saving vs ordinary-strength plate in large tankers, bulkers and container ships. See offshore platform steel plates when primary offshore grades apply.
Welding: higher-strength hull steels need approved higher-strength consumables matched to 0 °C weld-metal toughness; preheat and heat input follow the approved WPS and often track Ceq/Pcm from the mill certificate. TMCP AH40 must respect the Ceq caps noted above. Cutting by oxy-fuel/plasma/laser is routine; thick FH plate may need hydrogen control — follow mill recommendations.
Processing notes for BV AH40: cold forming is routine within normal shipyard radii. Line heating and fairing of TMCP plate should stay within the temperature limits recommended by the mill, because overheating can reduce the strength gained in controlled rolling. Check the delivery condition on the certificate before planning hot forming.
Certificates, BV survey and third-party inspection
Every plate is tested and marked at the mill under Bureau Veritas survey; the mill certificate lists heat number, ladle chemistry, Ceq where applicable, tensile results (ReH ≥ 390 N/mm², Rm 510–650 N/mm², A ≥ 20 %), Charpy at 0 °C, delivery condition and plate numbers, endorsed by the Surveyor. Optional EN 10204 3.2, UT (U), Z-direction, multi-class with ABS/DNV/LR.
On receipt: verify BV AH40 stamp, 0 °C impact data, energies for the delivered thickness band, thickness within UR W13 / PO tolerance, BV endorsement present.
Charpy acceptance for BV AH40 by thickness (IACS UR W11; actual results as per standard and mill certificate):
| Thickness t (mm) | Test temperature | Average energy, longitudinal (J min.) | Average energy, transverse (J min.) |
|---|---|---|---|
| t ≤ 50 | 0 °C | 39 | 26 |
| 50 < t ≤ 70 | 0 °C | 46 | 31 |
| 70 < t ≤ 100 | 0 °C | 55 | 37 |
If UT or 3.2 was ordered, check the UT report and inspector’s plate list as well.
Common mistakes when ordering BV AH40 / BV AH40
- Ordering “BV 40” without the letter (AH/…) — toughness class missing
- Accepting ordinary-strength Grade A/B certificates for a AH40 PO
- Ignoring TMCP Ceq caps on TM plate
- Substituting a different letter (e.g. AH for AH) without drawing approval
- Coil-cut plate without coil approval
- Missing BV endorsement on the MTC
- Writing DNV NV A40 or LR/AH40 on a BV-class PO without arranging that society’s survey
Write grade, delivery condition, impact temperature and certificate type into the PO.
Sourcing BV BV AH40: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Fake class plate | BV-approved mills only; traceable BV AH40 stamp + certificate; 3.2 on request |
| Payment risk | T/T or L/C; inspection before balance |
| Mixed sizes / grades | AH40 combined with BV Grade A/B/D/E or other AH–FH sizes in one container |
| Lead time visibility | weekly photo updates from dedicated coordinator |
| Prep before ship | cutting, bevelling, drilling, machining in our workshop |
How to order BV BV AH40 plate
Specify BV AH40 (BV AH40), delivery condition (AR/CR/N/TM/QT as applicable), thickness × width × length × qty, Z/U, multi-class, certificate type, port. Send to SHH STEEL.
Sample PO line: “Steel plate to Bureau Veritas NR216 Materials, Grade AH40 (BV AH40), delivery condition [AR/CR/N/TM/QT], 20 × 2500 × 12000 mm, 30 pcs, marked BV AH40 / BV AH40, certificate endorsed by BV Surveyor, EN 10204 3.2 [if required], UT [if required], CIF [port].”
FAQ
Conclusion
BV AH40 / BV AH40 is higher-strength hull steel under Bureau Veritas NR216 Materials rules and IACS UR W11: yield 390 N/mm², tensile 510–650 N/mm², Charpy at 0 °C, marking BV AH40. Lock on the order: delivery condition, impact lot size, TMCP Ceq if TM, product analysis if needed, multi-class and 3.2.
SHH STEEL supplies BV AH40 plate rolled by Chinese mills that hold Bureau Veritas works approval for the grade, so every plate carries the BV AH40 stamp and a Surveyor-endorsed certificate traceable to its heat. Common thicknesses are available from stock; other sizes are scheduled into the mill rolling cycle with BV survey arranged at the mill. On request we add EN 10204 3.2 certificates with third-party witness (TÜV, SGS, LR or another agency) and joint certification with ABS, DNV, LR, CCS, NK, KR or RINA.
We accept T/T or L/C payment, with inspection before the balance is paid. Small quantities in several sizes, or BV AH40 mixed with BV Grade A/B/D/E or other AH–FH sizes, can be combined in one container. A dedicated coordinator sends production and shipping updates with photos, and our own workshop cuts to size, bevels, drills and machines plates before shipment so they arrive ready for fabrication.
Request a quotation: send SHH STEEL the grade (BV AH40 / BV AH40), thickness, width, length, quantity per size and destination port, plus any multi-class, Z/U or 3.2 certificate requirement. We reply with price, available stock and lead time.