EN 10025-2 S355J2 Steel Plate | S355J2 Structural Steel - SHH STEEL

EN 10025-2 S355J2 Steel Plate | S355J2 Structural Steel

EN 10025-2 S355J2 is a high-strength non-alloy structural steel plate with a minimum yield strength of 355 MPa and impact tested at –20°C. It offers good weldability and excellent low-temperature toughness. SHH STEEL is a China Mill-Direct Exporter supplying S355J2 steel plate worldwide.
Equivalent Grades
ASTM A572 Gr 50 / JIS SM490A (-20℃) / GB Q355D / ISO E355D
Specification:
EN 10025-2 — Delivery: As-rolled or normalized rolling (N)
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Tolerances
Weldability
Equivalent Material Grades
Applications
Why Choose SHH STEEL
FAQ
Conclusion

What is EN 10025-2 S355J2 Steel Plate?

As a professional steel plate supplier and China Mill-Direct Exporter, SHH STEEL is pleased to present EN 10025-2 S355J2 Steel Plate (Material Number: 1.0577).

S355J2 is a high-strength non-alloy structural steel under the European standard EN 10025-2. It provides a minimum yield strength of 355 MPa (for thickness ≤ 16 mm) and is impact tested at –20°C with a minimum energy of 27 J. Compared with S355JR and S355J0, the lower impact test temperature makes S355J2 more suitable for structural applications in cold environments or where higher toughness is required. SHH STEEL sources this material directly from leading Chinese steel mills, ensuring competitive mill-direct pricing, stable quality and reliable delivery.

We supply S355J2 steel plate in thicknesses from 6 mm to 150 mm (thicker plates available on request), widths up to 3000–4000 mm, and lengths up to 12000–18000 mm. Custom cutting, shot blasting and priming services are available. All plates are delivered with full Mill Test Certificates (EN 10204 3.1).

Material Specification

EN 10025-2 S355J2 steel plate is produced in accordance with EN 10025-2.

Specification Element Requirement SHH STEEL Compliance
Primary Standard EN 10025-2 Full compliance
Steel Grade S355J2 (1.0577) Confirmed
Delivery Condition +AR (As-rolled) or +N (Normalized) Available
Product Form Steel Plate Available
Thickness Range 6 mm – 150 mm Custom sizes available
Width / Length Up to 3000–4000 mm / 12000–18000 mm Custom cutting supported
Certification EN 10204 3.1 / 3.2 Available

Chemical Composition

According to EN 10025-2, the chemical composition is specified for both ladle analysis (cast analysis) and product analysis.

Ladle Analysis (Cast Analysis)

Element Max. Limit (%)
Carbon (C) 0.20
Silicon (Si) 0.55
Manganese (Mn) 1.60
Phosphorus (P) 0.025
Sulfur (S) 0.025
Nitrogen (N) 0.012
Copper (Cu) 0.55

Product Analysis

Element Max. Limit (%)
Carbon (C) 0.23
Silicon (Si) 0.60
Manganese (Mn) 1.70
Phosphorus (P) 0.035
Sulfur (S) 0.035
Nitrogen (N) 0.014
Copper (Cu) 0.60

Note:

  • The maximum nitrogen content does not apply if the total aluminium content is ≥ 0.020%.
  • Carbon Equivalent (CEV) is controlled to ensure good weldability.
  • S355J2 is normally fully killed.

Mechanical Properties

Mechanical properties of EN 10025-2 S355J2 (longitudinal direction):

Thickness (mm) Yield Strength ReH (min) Tensile Strength Rm Elongation A (min) Impact Energy KV (min)
≤ 16 355 MPa 470 – 630 MPa 22% 27 J at –20°C
> 16 ≤ 40 345 MPa 470 – 630 MPa 22% 27 J at –20°C
> 40 ≤ 63 335 MPa 470 – 630 MPa 21% 27 J at –20°C
> 63 ≤ 100 325 MPa 470 – 630 MPa 20% 27 J at –20°C
> 100 ≤ 150 295 – 285 MPa 450 – 600 MPa 18% 27 J at –20°C

Delivery Conditions

SHH STEEL, as a China Mill-Direct Supplier, supplies EN 10025-2 S355J2 steel plate mainly in the following conditions:

  • +AR (As-rolled) – most common
  • +N (Normalized) – available on request

Additional options:

  • Shot blasting and shop primer
  • Ultrasonic testing (EN 10160)
  • Z-direction testing (Z15 / Z25 / Z35)
  • Third-party inspection (SGS, BV, TUV, etc.)

Tolerances

Dimensional tolerances for S355J2 steel plate follow EN 10029 (for plates) or EN 10051 (for strips).

  • Thickness, width and length tolerances according to the ordered class.
  • Flatness according to EN 10029.
  • Edge conditions: Mill edge or cut edge (flame / plasma).

Tighter tolerances can be provided upon request.

Weldability

S355J2 has good weldability. It can be welded by conventional methods (SMAW, SAW, GMAW, FCAW, etc.). Due to the higher strength and carbon equivalent, preheating is often recommended for thicker plates. Low-hydrogen consumables are advised for critical applications.

Equivalent Material Grades

Grade Standard Notes
S355J2 EN 10025-2 —
1.0577 EN Material number
Q355D GB/T 1591 Closest Chinese equivalent
A572 Grade 50 (approx.) ASTM Similar strength level
St52-3N DIN (old) Former designation

Applications

EN 10025-2 S355J2 is widely used in structural applications requiring high strength and good toughness at low temperatures. Typical uses include:

Application Area Typical Components / Uses (Keywords)
Building Structures Beams, columns, heavy frames – S355J2 Structural Steel
Bridges Bridge components in cold regions – S355J2 Bridge
Machinery Heavy equipment frames – S355J2 Machinery
Construction High-strength structures requiring –20°C toughness – S355J2 Construction
Offshore & Industrial Structural components – S355J2 Industrial
General Fabrication Welded high-strength structures – S355J2 Fabrication

Why Choose SHH STEEL

SHH STEEL is a China Mill-Direct Exporter. We maintain long-term strategic cooperation with major Chinese steel mills and act as a first-level (primary) agent. This direct mill supply model allows us to offer competitive mill-direct pricing, faster delivery times, stable and traceable quality, and full Mill Test Certificates (EN 10204 3.1 / 3.2) for EN 10025-2 S355J2 Steel Plate.

Customers benefit from reliable supply, short lead times and cost-effective solutions for structural steel projects worldwide. Our professional export team provides technical support and customized processing services to meet project requirements.

FAQ

What does the “J2” in S355J2 mean?
J2” indicates that the steel meets the impact energy requirement of minimum 27 J at –20°C.
What is the material number of S355J2?
1.0577
Can SHH STEEL supply normalized S355J2 (+N)?
Yes. Both as-rolled (+AR) and normalized (+N) conditions are available.

Conclusion

EN 10025-2 S355J2 (1.0577) Steel Plate from SHH STEEL offers high strength combined with excellent toughness at –20°C, making it ideal for demanding structural applications in cold environments. As a China Mill-Direct Exporter, we provide competitive pricing, fast delivery and consistent quality backed by full mill certifications. Trust SHH STEEL for your S355J2 structural steel plate requirements.

Contact SHH STEEL today for stock availability, pricing and technical support.

EN 10025-2 S355J2 Steel Plate, S355J2 steel plate, S355J2 structural steel, EN 10025 S355J2, S355J2 equivalent, S355J2 supplier, 1.0577

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X