ASTM A264 SA285 Gr.C + 304 Stainless Steel Clad Plate

ASTM A264 SA285 Gr.C + 304 stainless steel clad plate joins a type 304 layer to an SA285 Grade C carbon steel base. It is the economical stainless clad plate for storage tanks, hoppers and low-pressure vessels that need a clean stainless face. SHH STEEL produces it by explosion bonding with shear and UT tests on request.
Keywords
SA285 Gr.C + 304 clad plate, ASTM A264 304 clad plate, stainless clad tank plate, SA285 stainless steel clad plate, 304 clad carbon steel
Equivalent Grades:
ASME SA-264, GB/T 8165, JIS G3601; 304 = S30400 / 1.4301; SA285 Gr.C ≈ Q245R / SB410 (approx.)
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA285 Gr.C + 304 stainless steel clad plate?

ASTM A264 SA285 Gr.C + 304 stainless steel clad plate is a bimetal plate made of a type 304 (UNS S30400) austenitic stainless steel layer metallurgically bonded to an SA285 Grade C carbon steel base. The carbon steel carries the load; the 304 face meets the stored or processed product. It is ordered to ASTM A264 or the identical ASME version, SA-264.

On drawings it is written SA285 Gr.C + 304 with a thickness pair such as 3 + 10 mm. It is the budget stainless clad plate for atmospheric and low-pressure equipment: storage tanks, hoppers, silos and food and beverage vessels where a clean stainless face is needed, the design pressure is low and the vessel will not be stress relieved.

Compared with the SA516 Gr.70 version, the SA285 Grade C base is softer and cheaper, but it is limited in thickness and not meant for low-temperature or impact-tested service.

The question we hear most is whether to order 304 or 304L. The short answer: 304 has higher minimum strength, 304L is safer when the plate will be welded and heat treated. Much plate on the market is dual certified to both grades, but the order should still say which one is required.

SHH STEEL can produce 304 clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 304 clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA285 Gr.C + 304
Cladding A240 / SA-240 304, UNS S30400
Base steel A285 / SA-285 Grade C (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

A typical order line: “Clad plate to ASME SA-264, cladding SA-240 Type 304, 3 mm minimum; base SA-285 Grade C, 12 mm minimum; Class 3 bond quality; finish pickled.” If the vessel will receive PWHT, state it here: it changes the advice on the cladding grade.

SA285 Gr.C base and 304 cladding

The two layers of SA285 Gr.C + 304 are chosen for different jobs: SA285 Gr.C for code strength, toughness and weldability, 304 for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 304 is specified as the cladding

Type 304 (ASME SA240 304) has 18.0 to 20.0 % chromium, 8.0 to 11.0 % nickel and up to 0.08 % carbon. Compared with 304L it has a higher minimum yield strength, 205 against 170 MPa, and a higher minimum tensile strength, 515 against 485 MPa. That matters when the designer counts the cladding in the strength calculation, which A264 allows when the order says so.

The higher carbon is the trade-off. Held in the range of roughly 425 to 815 °C, 304 can form chromium carbides at grain boundaries and become prone to intergranular attack. Typical PWHT of a carbon steel vessel falls inside that range. For plates that will be stress relieved, we therefore suggest 304L or dual-certified 304/304L cladding; for vessels that are not heat treated and see mild media, 304 is a sound choice.

SA285 Grade C as the base steel

ASME SA285 Grade C is the strongest of the three A285 grades: a plain carbon pressure vessel plate with 380 to 515 MPa tensile strength and 205 MPa minimum yield, normally supplied as-rolled. A285 may be made by killed, semi-killed or rimmed practice at the producer’s option, and its thickness has traditionally been limited to 50 mm for internal soundness (recent editions word this differently, so check the edition on the order).

As a clad plate base it is the economical choice for low-pressure and atmospheric equipment, where wall thickness is set by minimum thickness rules or by stiffness rather than by stress. It is not intended for low-temperature service; where Charpy impact testing or fine-grain steel is required, SA516 is the base to use.

304, 304L and 304/304L dual-certified cladding

Cladding C max, % Min. yield / tensile, MPa Best fit
304 (S30400) 0.08 205 / 515 No PWHT, strength counted, mild media
304L (S30403) 0.030 170 / 485 Welded and stress relieved vessels
304/304L dual 0.030 205 / 515 Meets both grades; common mill practice
304LN 0.030 Higher, nitrogen strengthened Low carbon with strength close to 304

Explosion bonded and roll bonded 304 clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 304 plate is set above the SA285 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

For type 304 cladding, roll bonding is attractive on large, thin tank and hopper plates; explosion bonding covers heavy sections and small quantities.

Chemical composition of 304 cladding and SA285 Gr.C base

The chemical composition of SA285 Gr.C + 304 clad plate is certified layer by layer: the 304 cladding to ASTM A240 and the base to ASTM A285 / ASME SA-285.

304 cladding (UNS S30400)

Element 304 cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.08 max 0.01 over max ≤ 0.09
Manganese (Mn) 2.00 max 0.04 over max ≤ 2.04
Phosphorus (P) 0.045 max 0.010 over max ≤ 0.055
Sulfur (S) 0.030 max 0.005 over max ≤ 0.035
Silicon (Si) 0.75 max 0.05 over max ≤ 0.80
Chromium (Cr) 18.0 – 20.0 0.20 under min / 0.20 over max 17.80 – 20.20
Nickel (Ni) 8.0 – 11.0 0.15 under min / 0.15 over max 7.85 – 11.15
Nitrogen (N) 0.10 max 0.01 over max ≤ 0.11
Iron (Fe) Balance — —

These are the A240 limits for UNS S30400, with the A480 Table A1.1 tolerance applied below the minimum and above the maximum of each range. A dual-certified 304/304L cladding must satisfy the 0.030 % carbon limit of 304L and the strength of 304 at the same time.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA285 Grade C base steel

Element SA285 Gr.C heat analysis, % Product analysis, %
Carbon (C) 0.28 max 0.28 max
Manganese (Mn) 0.90 max 0.98 max
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Copper (Cu) 0.20 min when copper-bearing steel is specified —
Iron (Fe) Balance Balance

A285 sets no silicon range because the steel need not be killed. Carbon, phosphorus and sulfur limits apply to heat and product analysis alike.

Mechanical properties and bond strength of 304 clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 304 cladding (A240) SA285 Gr.C base
Tensile strength 515 MPa min 380 – 515 MPa
Yield strength (0.2 % offset) 205 MPa min 205 MPa min
Elongation 40 % min in 50 mm 27 % min in 50 mm; 23 % min in 200 mm
Hardness 201 HBW / 92 HRBW max Not specified

SA285 Gr.C has a minimum tensile strength of 380 MPa and a minimum yield of 205 MPa, both below the A264 thresholds, so a composite of 38 mm or less is tested full thickness. The acceptance range is 380 to 550 MPa: the base minimum up to its maximum plus 35 MPa. Type 304 is stronger than SA285 Gr.C, so the composite usually sits in the upper part of that range; for a 3 + 12 mm plate a result of about 400 to 450 MPa is typical (an estimate, not a requirement).

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. For storage tanks Class 3 or 5 is common; heads and tube sheets justify Class 1.

Thickness and toughness limits of the base

SA285 Gr.C plate has traditionally been limited to 50 mm, and the specification sets no impact test by default. Clad plates for this base are therefore ordered mostly in total thicknesses of 8 to 34 mm. If the design calls for Charpy testing, a minimum design metal temperature well below ambient, or thicker plate, change the base to SA516 Gr.70 rather than adding supplementary tests to SA285.

Heat treatment of SA285 Gr.C + 304 clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

As with other austenitic claddings, explosion bonded 304 plates are commonly supplied as-clad and flattened or stress relieved by agreement, and roll bonded plates in the mill’s heat treated condition. A full solution treatment restores the cladding but also affects the carbon steel, so it is agreed case by case.

If a 304 clad vessel must be post-weld heat treated, discuss it before ordering. Options are to switch to 304L or dual-certified cladding, to accept the risk where the medium is mild, or to specify an intergranular corrosion test after simulated PWHT.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

SA285 Gr.C is an as-rolled steel, so the clad plate is normally delivered as-clad and flattened. Its low carbon equivalent means post-weld heat treatment is often not required at the thicknesses used for tanks, which also suits the 304 cladding.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 304 cladding to a minimum thickness, normally 2 to 3 mm, so the design corrosion allowance is guaranteed. The 304 face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 304 clad plate

SA285 Gr.C + 304 clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 304; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 6 8 Light tanks and hoppers
2 + 8 10 Storage tanks
3 + 10 13 Tank shells
3 + 12 15 Low-pressure vessels
3 + 16 19 Tank bottoms and heads
4 + 20 24 Larger tanks
4 + 30 34 Heavier vessels
6 + 40 46 Near the A285 thickness range limit
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA285 Gr.C + 304 clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 304 surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA285 Gr.C side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a 309L type filler to absorb dilution from the carbon steel.
  5. Cap with 308 or 308L filler; 308L is the usual choice because it keeps weld-metal carbon low, then pickle and passivate the weld zone.

Even when the plate itself is type 304, many procedures use low-carbon 308L for the cap, so that the weld zone is no more sensitive than the cladding. Cutting is by plasma from the clad side, or oxy-fuel from the steel side on thick plates, with the cut face ground before welding.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

On the steel side, SA285 Gr.C welds easily with E7018 or ER70S-6 type filler and seldom needs preheat at normal thicknesses. Watch for laminations near the edges of semi-killed plate when preparing bevels; ultrasonic scanning of the bevel zone is a cheap precaution.

Applications of 304 stainless steel clad plate

304 stainless steel clad plate is used where a carbon steel structure needs a stainless face for hygiene, product purity or mild corrosion, and the vessel is not stress relieved.

  • Atmospheric storage tanks for water, edible oils, wine and spirits.
  • Food and beverage process and holding tanks.
  • Hoppers, silos and chutes needing a clean stainless face.
  • Hot water and low-pressure heater shells in low-chloride water.
  • Pulp and paper chests for non-chloride stock.
  • Low-pressure treaters and separators without impact requirements.

Stainless clad vs solid 304

Solid 304 is simpler in thin sections. Once the shell passes about 10 to 12 mm, a 304 clad steel plate usually costs less, and the carbon steel side is easier to weld to supports and nozzles made of carbon steel.

Why SA285 Gr.C as the base

SA285 Gr.C suits tanks and vessels with low design pressure where thickness is set by minimum rules, stiffness or corrosion allowance rather than stress. Its lower price and easy welding make the clad plate cheaper than the SA516 version, and 304’s general corrosion resistance matches the mild media typical of such equipment.

For pressurised vessels, low-temperature service or thicknesses over about 50 mm, use the SA516 Gr.70 + 304 pairing instead.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A285 and A240 304 Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Intergranular corrosion test after simulated PWHT ASTM A262 practice, by agreement When the vessel is stress relieved
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 304, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 304 UNS S30400 1.4301 (X5CrNi18-10) SUS304 06Cr19Ni10 (S30408)
Base A285 / SA-285 Grade C K02801 P235GH / P265GH (approx.) SB410 (approx.) Q245R (approx.)

In China the nearest product is GB/T 8165 S30408 on Q245R; in Japan, JIS G3601 SUS304 on SB410. These are close equivalents, not exact ones; check them against the design code.

Why order 304 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. With 304 enquiries we always ask whether the vessel will be stress relieved, because that single answer decides between 304, 304L and dual-certified cladding. For SA285 Gr.C orders we confirm that the design is within the base’s thickness and temperature range before production.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

What is the difference between 304 and 304L clad plate?
304 allows up to 0.08 % carbon and has 205/515 MPa minimum yield/tensile; 304L limits carbon to 0.030 % and has 170/485 MPa. 304L resists sensitization during welding and stress relief; 304 is stronger on paper.
Can I order dual-certified 304/304L cladding?
Yes. A cladding that meets both A240 grades combines low carbon with 304 strength. Write "SA-240 304/304L dual certified" on the order so the certificate shows both.
When should I choose SA285 Gr.C instead of SA516 Gr.70 as the base?
For atmospheric and low-pressure tanks and vessels without impact testing, where thickness is not set by stress. SA516 Gr.70 is the right base for higher pressure, low-temperature service or thick plate.
Which filler metals are used for SA285 Gr.C + 304?
Carbon steel filler for the base, a 309L buffer layer on the clad side and a 308L or 308 cap. Carbon steel filler must never be deposited on the cladding.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 304 cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA285 Gr.C + 304 Stainless Steel Clad Plate

ASTM A264 SA285 Gr.C + 304 stainless steel clad plate combines A240 type 304 cladding with an SA285 Grade C base, bonded by explosion or roll bonding, with 140 MPa minimum shear strength when specified and ultrasonic bond quality Class 1, 3 or 5. It is a cost-effective choice for tanks and vessels that are not stress relieved.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X