ASTM A264 SA516 Gr.70 + 316 Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 316 stainless steel clad plate bonds a type 316 molybdenum stainless layer to a carbon steel pressure vessel base. It resists chlorides and mild acids better than 304 at a fraction of solid stainless cost. SHH STEEL produces it by explosion or roll bonding, with 140 MPa bond shear and ultrasonic tests when ordered.
Keywords
316 stainless steel clad plate, ASTM A264 316 clad plate, SA516 Gr.70 + 316, 316 clad steel plate, molybdenum stainless clad plate
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; 316 = S31600 / 1.4401
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA516 Gr.70 + 316 stainless steel clad plate?

ASTM A264 SA516 Gr.70 + 316 stainless steel clad plate is a bimetal pressure vessel plate made of a 316 (UNS S31600) molybdenum-bearing austenitic stainless steel layer metallurgically bonded to an SA516 Grade 70 carbon steel base. The base steel carries pressure and structural load; the 316 face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

Drawings write it as SA516 Gr.70 + 316 with the thickness pair, such as 3 + 16 mm. Type 316 adds 2 to 3 % molybdenum to the 18-8 base, which is what lets it resist pitting and crevice attack in chloride-bearing water and many organic and dilute reducing acids where 304 fails.

Straight 316, as opposed to 316L, allows up to 0.08 % carbon. It is chosen when the vessel will not be stress relieved and a higher minimum yield is useful, or when the cladding is bought as 316/316L dual-certified material that meets both grades at once.

SHH STEEL can produce 316 clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 316 clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA516 Gr.70 + 316
Cladding A240 / SA-240 316, UNS S31600
Base steel A516 / SA-516 Grade 70 (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

A complete order line reads: “Clad plate to ASME SA-264, cladding SA-240 Type 316, 3 mm minimum; base SA-516 Grade 70, 16 mm minimum; Class 3 bond quality; shear test required; finish pickled.” If the vessel will be post-weld heat treated, consider ordering SA-240 316L or 316/316L dual-certified cladding instead, and state any intergranular corrosion test.

SA516 Gr.70 base and 316 cladding

The two layers of SA516 Gr.70 + 316 are chosen for different jobs: SA516 Gr.70 for code strength, toughness and weldability, 316 for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 316 is specified as the cladding

Type 316 (ASME SA240 316) contains 16.0 to 18.0 % chromium, 10.0 to 14.0 % nickel and 2.00 to 3.00 % molybdenum. The molybdenum raises the pitting resistance equivalent number to about 23 at minimum chemistry, compared with about 18 for 304, and broadens resistance to sulfurous, phosphoric and organic acids.

The higher carbon of 316 gives a minimum yield of 205 MPa, against 170 MPa for 316L. The cost is sensitization risk: held between roughly 425 and 815 °C, chromium carbides can form at grain boundaries and the cladding can then suffer intergranular corrosion in aggressive media.

SA516 Grade 70 as the base steel

ASME SA516 Grade 70 is a carbon-manganese-silicon vessel plate with 485 to 620 MPa tensile strength and 260 MPa minimum yield, supplied as-rolled or normalized and Charpy tested when the design temperature calls for it. Outside Code work the same steel is bought as ASTM A516 Grade 70; where a lower strength base is enough, ASME SA516 Grade 60 is used the same way.

316, 316L and 316/316L dual-certified cladding

Cladding C max, % Min. yield / tensile, MPa Best fit
316 (S31600) 0.08 205 / 515 No PWHT; strength counted; chloride water
316L (S31603) 0.030 170 / 485 Welded and stress relieved vessels
316/316L dual 0.030 205 / 515 Meets both grades; common mill practice
317L (S31703) 0.030 205 / 515 More chloride or acid than 316L can handle

Explosion bonded and roll bonded 316 clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 316 plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

Both explosion and roll bonding are used for 316 claddings. Roll bonding suits large, thin plates for tanks and hoppers; explosion bonding covers tube sheets, heavy sections and small quantities.

Chemical composition of 316 cladding and SA516 Gr.70 base

The chemical composition of SA516 Gr.70 + 316 clad plate is certified layer by layer: the 316 cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.

316 cladding (UNS S31600)

Element 316 cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.08 max 0.01 over max ≤ 0.09
Manganese (Mn) 2.00 max 0.04 over max ≤ 2.04
Phosphorus (P) 0.045 max 0.010 over max ≤ 0.055
Sulfur (S) 0.030 max 0.005 over max ≤ 0.035
Silicon (Si) 0.75 max 0.05 over max ≤ 0.80
Chromium (Cr) 16.0–18.0 0.20 under min / 0.20 over max 15.80–18.20
Nickel (Ni) 10.0–14.0 0.15 under min / 0.15 over max 9.85–14.15
Molybdenum (Mo) 2.00–3.00 0.10 under min / 0.10 over max 1.90–3.10
Nitrogen (N) 0.10 max 0.01 over max ≤ 0.11
Iron (Fe) Balance — —

These are the A240 limits for UNS S31600, with the A480 Table A1.1 tolerance applied below the minimum and above the maximum. Molybdenum is the line that makes 316 a 316: on product analysis it must stay at 1.90 % or above.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength of 316 clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 316 cladding (A240) SA516 Gr.70 base
Tensile strength 515 MPa min 485 – 620 MPa
Yield strength (0.2 % offset) 205 MPa min 260 MPa min
Elongation 40 % min in 50 mm 21 % min in 50 mm; 17 % min in 200 mm
Hardness 217 HBW / 95 HRBW max Not specified

A 3 + 16 mm SA516 Gr.70 + 316 plate is tested full thickness, and the composite must fall between 485 and 655 MPa. Type 316 and SA516 Gr.70 have similar tensile strength, so the composite lands comfortably in range.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Storage tanks and ducts are often ordered Class 3 or 5; heads and tube sheets justify Class 1.

Heat treatment of SA516 Gr.70 + 316 clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

Explosion bonded 316 plates are usually delivered as-clad and flattened, or stress relieved by agreement; roll bonded plates come through the mill’s own heat treatment. A full solution anneal of the cladding would also heat the SA516 base far above its intended treatment, so it is rarely used for clad plate.

If a 316 clad vessel must be post-weld heat treated, discuss it before ordering. The safer options are 316L or dual-certified cladding, or an intergranular corrosion test such as an ASTM A262 practice after a simulated PWHT under S3.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 316 cladding to a minimum thickness, usually 2 to 3 mm, so the corrosion allowance is guaranteed after any surface grinding. The 316 face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 316 clad plate

SA516 Gr.70 + 316 clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 316; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 8 10 Light tanks
2 + 10 12 Storage tanks
3 + 10 13 Low-pressure vessels
3 + 12 15 Vessel shells and heads
3 + 14 17 Process vessels
3 + 16 19 Columns, absorbers
3 + 20 23 Reactors, exchanger shells
3 + 25 28 Heavier shells
4 + 30 34 Heads
5 + 40 45 Small tube sheets
6 + 50 56 Tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA516 Gr.70 + 316 clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 316 surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA516 Gr.70 side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a 309L or 309MoL type filler, which tolerates dilution from the carbon steel.
  5. Cap with 316L filler, which keeps weld-metal carbon low and matches the molybdenum of the cladding, then pickle and passivate the weld zone.

For 316 cladding, 309MoL is a good buffer because it carries molybdenum into the first layer, and 316L caps restore the full surface chemistry. Using a low-carbon cap on a 316 cladding is normal practice: it lowers sensitization risk in the weld zone without any loss of corrosion resistance.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of 316 stainless steel clad plate

316 stainless steel clad plate is used where 304 would pit and the vessel is not post-weld heat treated.

  • Chemical process vessels handling dilute acids and chloride-bearing media.
  • Pulp and paper digesters and stock tanks.
  • Food and pharmaceutical tanks with salt or brine products.
  • Water and wastewater treatment vessels with moderate chlorides.
  • Storage tanks for fatty acids, organic acids and solvents.
  • Heat exchanger shells and channels on brackish cooling water.

When to move beyond 316

In warm seawater, strong chloride brines or hot sulfuric acid, 316 is likely to pit or corrode. Move to 317L, 904L, duplex 2205 or a nickel alloy; only the cladding changes, so the upgrade costs far less than in solid plate. See ASTM A264 for the other claddings.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A516 and A240 316 Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Intergranular corrosion test after simulated PWHT ASTM A262 practice, by agreement When the vessel is stress relieved
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 316, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 316 UNS S31600 1.4401 (X5CrNiMo17-12-2) SUS316 06Cr17Ni12Mo2 (S31608)
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Japanese projects order the same plate to JIS G3601 with SUS316 cladding; Chinese projects use GB/T 8165 or NB/T 47002.1 with S31608 on Q345R. The EN and GB grades are close substitutes, not identical, so check them against the design code.

Why order 316 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 316 orders we ask early whether the vessel will be stress relieved, because that decides between 316, 316L and dual-certified cladding.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

What is the difference between 316 and 316L clad plate?
316 allows up to 0.08 % carbon and has 205/515 MPa minimum yield/tensile; 316L limits carbon to 0.030 % and has 170/485 MPa. 316L resists sensitization during welding and PWHT; 316 is stronger. Dual-certified 316/316L meets both.
Is 316 clad plate suitable for seawater?
Only for limited exposure. Warm seawater can cause pitting and crevice corrosion of 316. For continuous seawater service, consider 2205, super austenitic, copper-nickel or titanium cladding.
Which filler metals are used for SA516 Gr.70 + 316?
Carbon steel filler for the base, a 309L or 309MoL buffer on the clad side, and a 316L cap.
Can 316 clad plate be post-weld heat treated?
It can, but the higher carbon of 316 increases sensitization risk. For PWHT vessels, 316L or 316/316L dual-certified cladding is the safer choice.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 316 cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA516 Gr.70 + 316 Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 316 stainless steel clad plate pairs an A240 type 316 layer with an SA516 Grade 70 base, bonded by explosion or roll bonding, with 140 MPa minimum shear strength when specified and ultrasonic bond Class 1, 3 or 5. It gives molybdenum-grade corrosion resistance for vessels that are not stress relieved.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X