ASTM A264 SA516 Gr.70 + 321 Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 321 stainless steel clad plate bonds titanium-stabilized 321 stainless steel to a carbon steel pressure vessel base. The stabilized cladding resists intergranular attack after exposure in the sensitizing range. SHH STEEL produces it by explosion or roll bonding, tested for 140 MPa bond shear and ultrasonic integrity when ordered.
Keywords
321 stainless steel clad plate, ASTM A264 321 clad plate, SA516 Gr.70 + 321, stabilized stainless clad plate, ASME SA 264
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; 321 = S32100 / 1.4541
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA516 Gr.70 + 321 stainless steel clad plate?

ASTM A264 SA516 Gr.70 + 321 stainless steel clad plate is a bimetal pressure vessel plate made of a 321 (UNS S32100) titanium-stabilized austenitic stainless steel layer metallurgically bonded to an SA516 Grade 70 carbon steel base. The base steel carries pressure and structural load; the 321 face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

It appears on drawings as SA516 Gr.70 + 321 with the thickness pair, for example 3 + 20 mm. Type 321 is an 18-10 austenitic stainless steel to which titanium is added at no less than five times the carbon plus nitrogen. The titanium ties up carbon as stable titanium carbides, so chromium stays in solution even after the steel has spent time between about 425 and 815 °C.

That property is why 321 is chosen for clad equipment that runs hot, cycles through the sensitizing range, or needs a cladding that will not be harmed by the base steel’s stress relief. It is also a long-standing alternative to 347 in refinery and petrochemical service.

SHH STEEL can produce 321 clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 321 clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA516 Gr.70 + 321
Cladding A240 / SA-240 321, UNS S32100
Base steel A516 / SA-516 Grade 70 (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

An order line reads: “Clad plate to ASME SA-264, cladding SA-240 Type 321, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1 bond quality, 100 % UT; shear test required; simulated PWHT per S3.” If a stabilizing heat treatment of the cladding is wanted, it must be agreed separately, because it is not a default of A264.

SA516 Gr.70 base and 321 cladding

The two layers of SA516 Gr.70 + 321 are chosen for different jobs: SA516 Gr.70 for code strength, toughness and weldability, 321 for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 321 is specified as the cladding

Type 321 (ASME SA240 321) carries 17.0 to 19.0 % chromium, 9.0 to 12.0 % nickel, up to 0.08 % carbon and titanium of at least 5 × (C + N), maximum 0.70 %. Unlike 304L, which avoids sensitization by having little carbon, 321 keeps its normal carbon and neutralizes it with titanium. The result is a cladding that resists intergranular corrosion after long exposure at temperature, not just after a short weld cycle.

321 also has good oxidation resistance and creep properties among the 18-8 grades, which is useful in heated vessels. Its general corrosion resistance is close to 304; it is not a substitute for 316L in chloride service.

SA516 Grade 70 as the base steel

ASME SA516 Grade 70 is a carbon-manganese-silicon vessel plate with 485 to 620 MPa tensile strength and 260 MPa minimum yield, supplied as-rolled or normalized and Charpy tested when the design temperature calls for it. Outside Code work the same steel is bought as ASTM A516 Grade 70; where a lower strength base is enough, ASME SA516 Grade 60 is used the same way.

321 compared with 347 and 304L

Cladding Stabilizer Typical reason to choose it
321 (S32100) Ti ≥ 5 × (C + N) Hot service and repeated heating in the sensitizing range
347 (S34700) Nb (columbium) Same duty; often preferred where welds must also be stabilized
304L (S30403) Low carbon only Short heat cycles, lower-temperature service
316L (S31603) Low carbon, Mo Chlorides and reducing acids

Explosion bonded and roll bonded 321 clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 321 plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

Both routes leave the titanium in the 321 layer untouched. Explosion bonding is common for the thick tube sheets and channel covers used in hot heat exchangers.

Chemical composition of 321 cladding and SA516 Gr.70 base

The chemical composition of SA516 Gr.70 + 321 clad plate is certified layer by layer: the 321 cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.

321 cladding (UNS S32100)

Element 321 cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.08 max 0.01 over max ≤ 0.09
Manganese (Mn) 2.00 max 0.04 over max ≤ 2.04
Phosphorus (P) 0.045 max 0.010 over max ≤ 0.055
Sulfur (S) 0.030 max 0.005 over max ≤ 0.035
Silicon (Si) 0.75 max 0.05 over max ≤ 0.80
Chromium (Cr) 17.0 – 19.0 0.20 under min / 0.20 over max 16.80 – 19.20
Nickel (Ni) 9.0 – 12.0 0.15 under min / 0.15 over max 8.85 – 12.15
Nitrogen (N) 0.10 max 0.01 over max ≤ 0.11
Titanium (Ti) 5 × (C + N) min, 0.70 max Ratio: product ≥ 0.90 × specified; 0.05 over max ≥ 4.5 × (C + N); ≤ 0.75
Iron (Fe) Balance — —

Limits are those of A240 for UNS S32100. For the titanium ratio, A480 accepts a product analysis down to 0.90 times the specified ratio, so the check value is 4.5 × (C + N). When reading a 321 certificate, compute the ratio from the reported carbon and nitrogen; a cladding that only just meets the titanium figure with high nitrogen may be under-stabilized.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength of 321 clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 321 cladding (A240) SA516 Gr.70 base
Tensile strength 515 MPa min 485 – 620 MPa
Yield strength (0.2 % offset) 205 MPa min 260 MPa min
Elongation 40 % min in 50 mm 21 % min in 50 mm; 17 % min in 200 mm
Hardness 217 HBW / 95 HRBW max Not specified

A 3 + 20 mm plate is tested full thickness, with the composite between 485 and 655 MPa. For hot service, remember that A264 only tests at room temperature; elevated-temperature design values come from the code tables for the base steel.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. For hot exchanger tube sheets we suggest Class 1 with 100 % coverage, since thermal cycling punishes any unbonded area.

Heat treatment of SA516 Gr.70 + 321 clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

A264’s default is a solution treatment of the austenitic cladding, but explosion bonded 321 plates are frequently delivered as-clad and flattened, or stress relieved, by agreement. Because 321 is stabilized, the SA516 base steel’s stress relief and the vessel’s PWHT do not sensitize the cladding the way they can with 304.

Some refinery specifications ask for a stabilizing heat treatment of 321 or 347 surfaces, aimed at polythionic acid stress corrosion during shutdowns. On clad plate this temperature affects the carbon steel base too, so it must be agreed with the manufacturer and covered by S3 coupons.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 321 layer to a minimum thickness, typically 3 mm, so that design corrosion allowance and oxidation margin are both protected. The 321 face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 321 clad plate

SA516 Gr.70 + 321 clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 321; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
3 + 12 15 Heated process vessels
3 + 14 17 Flue gas and exhaust ducts
3 + 16 19 Exchanger shells
3 + 20 23 Reactors and columns
3 + 25 28 Heavier shells
4 + 30 34 Channel heads
5 + 40 45 Tube sheets
6 + 50 56 Clad tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA516 Gr.70 + 321 clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 321 surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA516 Gr.70 side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a 309L type filler over the carbon steel weld metal.
  5. Cap with 347 type filler, because titanium does not transfer well across the welding arc and niobium-stabilized 347 filler gives a stabilized deposit, then pickle and passivate the weld zone.

The use of 347 filler on 321 cladding surprises some buyers, but it is normal practice: most of the titanium in a 321 electrode would be lost to oxidation in the arc. Keep interpass temperatures moderate and avoid heavy weaving, which raises heat input and dilution.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of 321 stainless steel clad plate

321 stainless steel clad plate goes into equipment where the cladding sees heat, either continuously or in cycles, and a stabilized grade is specified.

  • Heated reactors and process vessels in petrochemical plants.
  • Heat exchanger shells, channels and tube sheets in hot service.
  • Flue gas, exhaust and hot air ducts made from clad plate.
  • Refinery equipment where a stabilized grade is specified against intergranular attack.
  • Chemical vessels that are steam cleaned or regenerated at temperature.
  • Dryers and kilns with a stainless contact face.

Service temperature of 321 clad plate

The 321 layer tolerates higher temperatures than the SA516 Gr.70 base. The allowable stress tables of the design code for the base steel, and the risk of graphitization in long hot service, set the real limit. For higher temperatures, a Cr-Mo base such as ASTM A387 Grade 11 Class 2 replaces the carbon steel.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A516 and A240 321 Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Intergranular corrosion test of cladding ASTM A262 practice, by agreement When ordered
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 321, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 321 UNS S32100 1.4541 (X6CrNiTi18-10) SUS321 06Cr18Ni11Ti (S32168)
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

In China the cladding is S32168, ordered under GB/T 8165 or NB/T 47002.1; in Japan, SUS321 under JIS G3601. The EN, JIS and GB grades are close substitutes; confirm them against the design code.

Why order 321 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 321 work we check the titanium-to-carbon-plus-nitrogen ratio on every cladding certificate before bonding.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

What is the difference between 321 and 347 clad plate?
Both are stabilized 18-10 grades. 321 uses titanium, 347 uses niobium. They are used for the same hot or cycling duties; 347 is sometimes preferred because its welds match the base chemistry.
Why is 347 filler used to weld 321 cladding?
Titanium oxidizes in the arc and is largely lost, so a 321 filler would give an under-stabilized weld. Niobium in 347 filler survives the arc and stabilizes the deposit.
Is 321 better than 304L for PWHT?
For long or repeated heat treatment, yes. 304L relies on low carbon and resists short cycles; 321 neutralizes carbon with titanium and resists long exposure in the sensitizing range.
What is the Ti requirement for 321 cladding?
A240 requires titanium of at least 5 × (C + N) and no more than 0.70 %. On product analysis A480 accepts 4.5 × (C + N) and 0.75 % maximum.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 321 cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA516 Gr.70 + 321 Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 321 stainless steel clad plate combines titanium-stabilized A240 type 321 cladding with an SA516 Grade 70 base, with 140 MPa minimum shear strength when specified and ultrasonic bond quality Class 1, 3 or 5. It is the clad choice for hot and thermally cycled equipment.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X