ASTM A264 SA516 Gr.70 + 254SMO (S31254) Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 254SMO clad plate bonds UNS S31254, a 6 % molybdenum super austenitic stainless steel, to a carbon steel pressure vessel base. It resists pitting and crevice corrosion in seawater, brines and bleach plant liquors at a fraction of solid alloy cost. SHH STEEL produces it by explosion bonding with shear and UT tests.
Keywords
254SMO clad plate, S31254 clad plate, ASTM A264 254SMO, SA516 Gr.70 + S31254, 6Mo super austenitic clad plate
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; 254SMO = S31254 / 1.4547
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA516 Gr.70 + 254SMO stainless steel clad plate?

ASTM A264 SA516 Gr.70 + 254SMO stainless steel clad plate is a bimetal pressure vessel plate made of a 254SMO (UNS S31254) 6 % molybdenum super austenitic stainless steel layer metallurgically bonded to an SA516 Grade 70 carbon steel base. The base steel carries pressure and structural load; the 254SMO face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

It is written SA516 Gr.70 + S31254 or SA516 Gr.70 + 254SMO with the thickness pair. 254SMO is the best-known 6Mo super austenitic stainless steel: 20 % chromium, 18 % nickel, 6 to 6.5 % molybdenum, copper and nitrogen. Its pitting resistance is in the range of super duplex steels, while its austenitic structure makes it tough and relatively easy to fabricate.

As a cladding it serves seawater, brines and chlorine dioxide bleach liquors, where 316L and 317L fail and where nickel alloys would be more than the duty needs.

SHH STEEL can produce 254SMO clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 254SMO clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA516 Gr.70 + 254SMO
Cladding A240 / SA-240 254SMO, UNS S31254
Base steel A516 / SA-516 Grade 70 (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

A complete order line reads: “Clad plate to ASME SA-264, cladding SA-240 UNS S31254, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1, 100 % UT (S12); shear test required; G48 pitting test of cladding as agreed.”

SA516 Gr.70 base and 254SMO cladding

The two layers of SA516 Gr.70 + 254SMO are chosen for different jobs: SA516 Gr.70 for code strength, toughness and weldability, 254SMO for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 254SMO is specified as the cladding

S31254 (ASME SA240 S31254) contains 19.5 to 20.5 % chromium, 17.5 to 18.5 % nickel, 6.0 to 6.5 % molybdenum, 0.50 to 1.00 % copper and 0.18 to 0.25 % nitrogen, with carbon held to 0.020 %. Its PREN is about 42 at minimum chemistry, roughly double that of 316L.

Nitrogen raises strength as well as pitting resistance: A240 plate has a minimum yield of 310 MPa. The main metallurgical caution is that high molybdenum segregates in welds, so matching filler is not used; nickel-base fillers with more molybdenum are.

SA516 Grade 70 as the base steel

ASME SA516 Grade 70 is a carbon-manganese-silicon vessel plate with 485 to 620 MPa tensile strength and 260 MPa minimum yield, supplied as-rolled or normalized and Charpy tested when the design temperature calls for it. Outside Code work the same steel is bought as ASTM A516 Grade 70; where a lower strength base is enough, ASME SA516 Grade 60 is used the same way.

254SMO compared with neighbouring claddings

Cladding Mo, % Approx. PREN (min.) Choose it when
317L (S31703) 3.0 – 4.0 28 FGD, contaminated acids
904L (N08904) 4.0 – 5.0 32 Sulfuric acid
254SMO (S31254) 6.0 – 6.5 42 Seawater, bleach plants, brines
2507 (S32750) 3.0 – 5.0 41 Seawater where strength and SCC resistance are needed

Explosion bonded and roll bonded 254SMO clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 254SMO plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

254SMO is explosion bonded, usually in 2 to 4 mm claddings. Sheet is solution annealed before bonding.

Chemical composition of 254SMO cladding and SA516 Gr.70 base

The chemical composition of SA516 Gr.70 + 254SMO clad plate is certified layer by layer: the 254SMO cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.

254SMO cladding (UNS S31254)

Element 254SMO cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.020 max 0.005 over max ≤ 0.025
Manganese (Mn) 1.00 max 0.03 over max ≤ 1.03
Phosphorus (P) 0.030 max 0.005 over max ≤ 0.035
Sulfur (S) 0.010 max 0.005 over max ≤ 0.015
Silicon (Si) 0.80 max 0.05 over max ≤ 0.85
Chromium (Cr) 19.5 – 20.5 0.25 under min / 0.25 over max 19.25 – 20.75
Nickel (Ni) 17.5 – 18.5 0.15 under min / 0.15 over max 17.35 – 18.65
Molybdenum (Mo) 6.0 – 6.5 0.10 under min / 0.10 over max 5.90 – 6.60
Copper (Cu) 0.50 – 1.00 0.05 under min / 0.05 over max 0.45 – 1.05
Nitrogen (N) 0.18 – 0.25 0.02 under min / 0.02 over max 0.16 – 0.27
Iron (Fe) Balance — —

These are the A240 limits for UNS S31254, with A480 product tolerances worked out from the maximum of each range. Molybdenum, nitrogen and the very low carbon are the lines that define the grade.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength of 254SMO clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 254SMO cladding (A240) SA516 Gr.70 base
Tensile strength 655 MPa min (plate) 485 – 620 MPa
Yield strength (0.2 % offset) 310 MPa min 260 MPa min
Elongation 35 % min in 50 mm 21 % min in 50 mm; 17 % min in 200 mm
Hardness 223 HBW / 96 HRBW max Not specified

254SMO is stronger than SA516 Gr.70. A 3 + 20 mm plate tested full thickness must still fall between 485 and 655 MPa; with normal cladding ratios it does.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Seawater and bleach plant equipment is normally ordered Class 1 with 100 % coverage.

Heat treatment of SA516 Gr.70 + 254SMO clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

254SMO clad plate is delivered as-clad and flattened, or stress relieved by agreement. A full solution anneal of the composite is rarely practical.

High-molybdenum austenitics can precipitate intermetallic phases after long exposure at intermediate temperatures. Normal SA516 PWHT is short, but qualify it on S3 coupons with a G48 test where the service is critical.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 254SMO cladding to a minimum thickness, typically 2 or 3 mm. The 254SMO face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 254SMO clad plate

SA516 Gr.70 + 254SMO clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 254SMO; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 8 10 Light tanks
2 + 10 12 Storage tanks
3 + 10 13 Low-pressure vessels
3 + 12 15 Vessel shells and heads
3 + 14 17 Process vessels
3 + 16 19 Columns, absorbers
3 + 20 23 Reactors, exchanger shells
3 + 25 28 Heavier shells
4 + 30 34 Heads
5 + 40 45 Small tube sheets
6 + 50 56 Tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA516 Gr.70 + 254SMO clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 254SMO surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA516 Gr.70 side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a nickel-base filler such as ERNiCrMo-3.
  5. Cap with ERNiCrMo-3 or ERNiCrMo-4, over-alloyed in molybdenum relative to the cladding, then pickle and passivate the weld zone.

Matching 254SMO filler is not used, because molybdenum segregation leaves the weld metal less resistant than the plate. Nickel-base fillers with 9 % or more molybdenum restore full corrosion resistance; the same filler serves as buffer and cap.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of 254SMO clad plate

254SMO clad plate is used where chlorides are too severe for 316L or 317L.

  • Seawater coolers, filters and desalination vessels.
  • Pulp and paper chlorine dioxide bleach towers and washers.
  • FGD absorbers with high chloride levels.
  • Chemical processing of chloride-bearing acids.
  • Food processing with brines and salt.
  • Offshore process vessels on seawater duty.

254SMO clad plate vs solid 254SMO

Solid 6Mo plate is costly in heavy sections. A clad plate keeps the 6Mo layer where the fluid is and uses steel for the structure.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A516 and A240 254SMO Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Pitting corrosion test of cladding ASTM G48, by agreement When ordered
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 254SMO, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 254SMO UNS S31254 1.4547 (X1CrNiMoCuN20-18-7) SUS312L 015Cr20Ni18Mo6CuN (S31252)
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Japanese projects order it to JIS G3601; Chinese projects to GB/T 8165. Check equivalents against the design code.

Why order 254SMO clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 254SMO we confirm the filler and the G48 test conditions with the fabricator.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

What is 254SMO clad plate used for?
Seawater equipment, bleach plant towers, FGD absorbers and brine vessels where 316L and 317L pit.
Why are nickel alloy fillers used on 254SMO cladding?
Molybdenum segregates in matching weld metal, making it less resistant than the plate. ERNiCrMo-3 or -4 fillers restore resistance.
What is the PREN of 254SMO?
About 42 at minimum chemistry.
Is 254SMO stronger than 316L?
Yes. A240 plate has 655 MPa minimum tensile and 310 MPa minimum yield, against 485 and 170 MPa for 316L.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 254SMO cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA516 Gr.70 + 254SMO (S31254) Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 254SMO stainless steel clad plate combines S31254 6Mo super austenitic steel with an SA516 Grade 70 base, with 140 MPa shear when specified and ultrasonic Class 1, 3 or 5. It is the austenitic clad choice for seawater, bleach and brine service.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X