ASTM A264 SA516 Gr.60 + 316L Stainless Steel Clad Plate
What is ASTM A264 SA516 Gr.60 + 316L stainless steel clad plate?
ASTM A264 SA516 Gr.60 + 316L stainless steel clad plate is a bimetal pressure vessel plate made of a 316L (UNS S31603) low-carbon molybdenum austenitic stainless steel layer metallurgically bonded to an SA516 Grade 60 carbon steel base. The base steel carries pressure and structural load; the 316L face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.
It is written SA516 Gr.60 + 316L with the thickness pair, such as 3 + 14 mm. The cladding is the familiar 316L, with 2 to 3 % molybdenum and 0.030 % maximum carbon; what changes compared with the more common SA516 Gr.70 version is the base. Grade 60 has 415 to 550 MPa tensile strength and 220 MPa minimum yield, against 485 to 620 and 260 MPa for Grade 70.
Designers pick Grade 60 when pressure is modest and wall thickness is set by minimum thickness rules rather than stress, when heads are deep drawn or cold formed, or when low-temperature toughness is a priority, because the lower carbon helps impact properties.
SHH STEEL can produce 316L clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.
ASTM A264 / ASME SA-264 requirements for 316L clad plate
ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.
| Item | Requirement for SA516 Gr.60 + 316L |
|---|---|
| Cladding | A240 / SA-240 316L, UNS S31603 |
| Base steel | A516 / SA-516 Grade 60 (other carbon or low-alloy pressure vessel steels by agreement) |
| Bonding | Explosion bonding, hot roll bonding, or any process that meets A264 |
| General requirements | A20/A20M for the base; A480/A480M for cladding product analysis |
| Bond strength | 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them |
| Bond integrity | Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5 |
| Cladding finish | Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned |
| Marking | Base steel marking per A20 plus the cladding type and the specification number |
A complete order line reads: “Clad plate to ASME SA-264, cladding SA-240 316L, 3 mm minimum; base SA-516 Grade 60, normalized, 14 mm minimum; Class 3 bond quality; shear test required.” Add impact test requirements for the base if the minimum design metal temperature needs them.
SA516 Gr.60 base and 316L cladding
The two layers of SA516 Gr.60 + 316L are chosen for different jobs: SA516 Gr.60 for code strength, toughness and weldability, 316L for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.
Why 316L is specified as the cladding
316L (ASME SA240 316L) contains 16.0 to 18.0 % chromium, 10.0 to 14.0 % nickel and 2.00 to 3.00 % molybdenum, with carbon limited to 0.030 %. It resists chlorides and dilute acids better than 304L and goes through welding and stress relief without sensitization.
Paired with Grade 60, the clad plate is a little less strong but a little easier to form and weld than the Grade 70 version. For a detailed look at the cladding itself, see our SA516 Gr.70 + 316L page.
SA516 Grade 60 as the base steel
ASME SA516 Grade 60 is the lower-strength member of the A516 family: 415 to 550 MPa tensile strength and 220 MPa minimum yield, with lower carbon than Grade 70 and correspondingly easier welding and forming. It is supplied as-rolled or normalized and can be impact tested for low design temperatures.
Grade 60 is chosen as a clad plate base when the design pressure is modest, when heavy cold forming of heads is planned, or when the owner’s specification prefers a lower-carbon, tougher base. If a thinner shell is wanted, SA516 Grade 70 gives about 18 % more allowable stress.
SA516 Grade 60 vs Grade 70 as the base for 316L
| Property | SA516 Gr.60 | SA516 Gr.70 |
|---|---|---|
| Tensile strength | 415 – 550 MPa | 485 – 620 MPa |
| Yield strength, min | 220 MPa | 260 MPa |
| Elongation in 50 mm, min | 25 % | 21 % |
| Carbon max, 12.5 to 50 mm | 0.23 % | 0.28 % |
| Typical choice | Moderate pressure, formed heads, toughness | Higher pressure, thinner walls |
Explosion bonded and roll bonded 316L clad plate
Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.
Explosion bonding
The 316L plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.
Hot roll bonding
Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.
| Point | Explosion bonded | Roll bonded |
|---|---|---|
| Bond | Solid-state collision weld, wavy interface | Diffusion bond formed in the mill |
| Best suited to | Thick plates, tube sheets, project quantities | Large plates, thin claddings, repeat volumes |
| Base steel | Bought to its own specification before bonding | Properties result from rolling and heat treatment of the pack |
| Delivery forms | Plates, discs, head and tube sheet blanks | Plates and wide plates |
Both explosion and roll bonding suit SA516 Gr.60 + 316L. The lower-strength base bonds and flattens easily.
Chemical composition of 316L cladding and SA516 Gr.60 base
The chemical composition of SA516 Gr.60 + 316L clad plate is certified layer by layer: the 316L cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.
316L cladding (UNS S31603)
| Element | 316L cladding, heat analysis (A240), % | A480 Table A1.1 tolerance, % | Product analysis limit, % |
|---|---|---|---|
| Carbon (C) | 0.030 max | 0.005 over max | ≤ 0.035 |
| Manganese (Mn) | 2.00 max | 0.04 over max | ≤ 2.04 |
| Phosphorus (P) | 0.045 max | 0.010 over max | ≤ 0.055 |
| Sulfur (S) | 0.030 max | 0.005 over max | ≤ 0.035 |
| Silicon (Si) | 0.75 max | 0.05 over max | ≤ 0.80 |
| Chromium (Cr) | 16.0–18.0 | 0.20 under min / 0.20 over max | 15.80–18.20 |
| Nickel (Ni) | 10.0–14.0 | 0.15 under min / 0.15 over max | 9.85–14.15 |
| Molybdenum (Mo) | 2.00–3.00 | 0.10 under min / 0.10 over max | 1.90–3.10 |
| Nitrogen (N) | 0.10 max | 0.01 over max | ≤ 0.11 |
| Iron (Fe) | Balance | — | — |
These are the A240 limits for UNS S31603 with A480 product tolerances. Carbon (0.035 % max on product analysis) and molybdenum (1.90 % min) are the lines to check.
Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.
SA516 Grade 60 base steel
| Element | SA516 Gr.60 heat analysis, % | SA516 Gr.60 product analysis, % |
|---|---|---|
| Carbon (C), 12.5 mm and under | 0.21 max | 0.21 max |
| Carbon (C), over 12.5 to 50 mm | 0.23 max | 0.23 max |
| Carbon (C), over 50 to 100 mm | 0.25 max | 0.25 max |
| Carbon (C), over 100 mm | 0.27 max | 0.27 max |
| Manganese (Mn), 12.5 mm and under | 0.60 – 0.90 | 0.55 – 0.98 |
| Manganese (Mn), over 12.5 mm | 0.85 – 1.20 | 0.79 – 1.30 |
| Phosphorus (P) | 0.025 max | 0.025 max |
| Sulfur (S) | 0.025 max | 0.025 max |
| Silicon (Si) | 0.15 – 0.40 | 0.13 – 0.45 |
| Iron (Fe) | Balance | Balance |
Grade 60 plates 12.5 mm and under may also have 0.85 to 1.20 % manganese by heat analysis. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.
Mechanical properties and bond strength of 316L clad plate
Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.
Tensile test rules in ASTM A264
| Condition | Tensile test | Acceptance |
|---|---|---|
| Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less | Full-thickness composite specimen | Base steel minimum up to base steel maximum plus 35 MPa |
| Composite over 38 mm, or stronger base steel | Base steel only | All base steel tensile requirements |
| Cladding ordered as corrosion allowance only | Cladding need not be included | All base steel tensile requirements |
Properties of the two layers
| Property | 316L cladding (A240) | SA516 Gr.60 base |
|---|---|---|
| Tensile strength | 485 MPa min | 415 – 550 MPa |
| Yield strength (0.2 % offset) | 170 MPa min | 220 MPa min |
| Elongation | 40 % min in 50 mm | 25 % min in 50 mm; 21 % min in 200 mm |
| Hardness | 217 HBW / 95 HRBW max | Not specified |
SA516 Gr.60 has a minimum tensile strength below 485 MPa and a minimum yield below 275 MPa, so a composite of 38 mm or less is tested full thickness. The acceptance range is then 415 to 585 MPa: the Grade 60 minimum up to its maximum plus 35 MPa. 316L is slightly stronger than Grade 60, so the composite tends to sit in the upper part of that range; mill certificates of both layers help predict it.
Bond shear and bend tests
When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.
Ultrasonic bond quality classes
| Class | Largest single unbonded area | Total unbonded area |
|---|---|---|
| Class 1 | 25 mm (1 in) longest dimension | 1 % of clad surface |
| Class 3 | 75 mm (3 in) longest dimension | 3 % of clad surface |
| Class 5 | 58 cm² (9 in²) | 5 % of clad surface |
Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Class 3 is common for tanks and shells; heads and tube sheets justify Class 1.
Heat treatment of SA516 Gr.60 + 316L clad plate
Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.
SA516 Gr.60 + 316L plate is supplied as-clad and flattened, stress relieved, or with the base normalized where the order requires it. The low carbon of 316L tolerates these cycles and the vessel’s PWHT.
If the base must be normalized for impact properties, state it on the order so the bonding sequence can be planned.
Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.
Thickness tolerances and surface finish
Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.
| Item | ASTM A264 requirement |
|---|---|
| Ordered to minimum thickness | Cladding, base and total not below the ordered minimums |
| Nominal: base steel or total composite | 0.3 mm under |
| Nominal: cladding | 0.8 mm under |
| Over-tolerance of the total | Greater of 3 mm or 10 % of the ordered total, provided each minimum is met |
| Width, length, flatness | ASTM A20/A20M |
Order the 316L cladding to a minimum thickness, typically 2 or 3 mm. The 316L face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.
Stock sizes and thickness combinations of 316L clad plate
SA516 Gr.60 + 316L clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 316L; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.
| Cladding + base, mm | Total, mm | Typical use |
|---|---|---|
| 2 + 8 | 10 | Light tanks |
| 2 + 10 | 12 | Storage tanks |
| 3 + 10 | 13 | Low-pressure vessels |
| 3 + 12 | 15 | Formed heads |
| 3 + 14 | 17 | Vessel shells |
| 3 + 16 | 19 | Columns |
| 3 + 20 | 23 | Process vessels |
| 4 + 25 | 29 | Heads |
| 5 + 30 | 35 | Small tube sheets |
| 6 + 40 | 46 | Tube sheets |
| 8 + 50 and over | 58 and over | Large tube sheets |
| Dimension | Production range |
|---|---|
| Cladding thickness | 2 mm to 20 mm (thicker by explosion bonding on request) |
| Base steel thickness | 6 mm to 200 mm |
| Total thickness | 8 mm to 220 mm |
| Width | 1000 mm to 3000 mm; wider by explosion bonding with welded cladding |
| Length | 2000 mm to 12000 mm |
| Discs and blanks | Round tube sheet blanks and head blanks cut to drawing |
| Location | China |
Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.
Welding SA516 Gr.60 + 316L clad plate
A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 316L surface. Carbon steel filler must never land on the cladding.
- Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
- Weld the SA516 Gr.60 side with matching carbon steel filler.
- Back-gouge from the clad side to sound carbon steel weld metal.
- Deposit the transition layer with a 309L or 309MoL type filler.
- Cap with 316L filler, then pickle and passivate the weld zone.
Grade 60’s lower carbon makes the steel side easier to weld; preheat is rarely needed in normal thicknesses. On the clad side, 309MoL buffer and 316L caps are standard.
Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.
Applications of SA516 Gr.60 + 316L clad plate
SA516 Gr.60 + 316L clad plate is used for moderate-pressure vessels that need 316L on the process side.
- Chemical storage tanks and low-pressure process vessels.
- Deep-drawn and cold-formed heads.
- Low-temperature vessels where base toughness is a priority.
- Food and pharmaceutical vessels with brine or chloride products.
- Water treatment vessels.
- Heat exchanger shells on brackish water.
When to choose Grade 70 instead
If wall thickness is set by stress, SA516 Gr.70 gives a thinner, lighter shell. The cladding and welding are the same; only the base changes.
Testing and certification
An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.
| Test or document | Basis | Frequency / note |
|---|---|---|
| Chemical analysis of both layers | A516 and A240 316L | Each heat; product analysis if ordered |
| Tensile test | A264 and the base specification | Each plate as rolled |
| Shear test or three bond bend tests | A264 | When specified |
| Ultrasonic bond inspection | A578/A578M procedures, Class 1/3/5 | 10 mm and thicker; 100 % with S12 |
| Charpy V-notch impact | Supplementary Requirement S5 | When ordered for the base |
| Simulated PWHT of coupons | Supplementary Requirement S3 | When the vessel is heat treated |
| Charpy V-notch test of base at MDMT | A20/A20M, by agreement | When ordered |
| Visual and dimensional check | A20 and the order | Each plate |
| Mill test certificate | EN 10204 3.1; 3.2 with third-party inspection on request | Each plate or lot |
Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 316L, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.
Equivalent standards and grades
Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.
| Standard | Scope | Bond shear requirement | Bond quality levels |
|---|---|---|---|
| ASTM A264 / ASME SA-264 | Stainless chromium-nickel steel-clad plate | 140 MPa min, when specified | Class 1 / 3 / 5 |
| JIS G3601 | Stainless clad steels | 200 N/mm² min | Per JIS G3601 |
| GB/T 8165 | Stainless steel clad plate, sheet and strip (2025 edition) | 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) | Grades 1 / 2 / 3 |
| NB/T 47002.1 | Clad plate for pressure equipment, stainless steel-steel | Per NB/T 47002.1 | Per NB/T 47002.1 |
| Layer | ASTM / ASME | UNS | EN | JIS | GB |
|---|---|---|---|---|---|
| Cladding | A240 / SA-240 316L | UNS S31603 | 1.4404 (X2CrNiMo17-12-2) | SUS316L | 022Cr17Ni12Mo2 (S31603) |
| Base | A516 / SA-516 Grade 60 | K02100 | P265GH (approx.) | SGV410 (approx.) | GB/T 713 Q245R (approx.) |
Chinese projects order the nearest equivalent as S31603 + Q245R to GB/T 8165; Japanese projects use JIS G3601 with SUS316L. Check equivalents against the design code.
Why order 316L clad plate from SHH STEEL
SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For Grade 60 orders we confirm normalizing and impact requirements of the base before production.
- We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
- We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
- Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
- Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.
FAQ
-
Why use SA516 Gr.60 instead of Gr.70 for 316L clad plate?
- Grade 60 has lower carbon and strength, which helps forming, welding and toughness. It suits moderate-pressure vessels; Grade 70 allows thinner walls at higher pressure.
-
How is SA516 Gr.60 + 316L tensile tested?
- Up to 38 mm composite thickness, full thickness; acceptance is 415 MPa up to 585 MPa (the Grade 60 maximum plus 35 MPa).
-
Which filler metals weld SA516 Gr.60 + 316L?
- Carbon steel filler for the base, a 309L or 309MoL buffer and 316L caps.
-
Can SA516 Gr.60 + 316L be impact tested?
- Yes. Charpy tests of the base are ordered under A20/A20M at the design temperature.
-
Is ASME SA-264 the same as ASTM A264?
- Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
-
What is the HS code for stainless steel clad plate?
- Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
-
What should I send for a quotation?
- The standard (ASTM A264 or ASME SA-264), 316L cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.
Request a quotation for ASTM A264 SA516 Gr.60 + 316L Stainless Steel Clad Plate
ASTM A264 SA516 Gr.60 + 316L stainless steel clad plate combines A240 316L with the lower-strength, lower-carbon SA516 Grade 60 base, with 140 MPa shear when specified and ultrasonic Class 1, 3 or 5. It suits moderate-pressure vessels, formed heads and low-temperature service.
Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.
Contact: admin@steelspecs.com