Q420MC TMCP Steel Plate GB/T 1591 Supplier
What is Q420MC TMCP Steel Plate GB/T 1591?
Q420MC, also searched as GB/T 1591 Q420MC, Q420MC steel plate, Q420MC TMCP plate and Q420 MC, is the 420 MPa quality-grade-C grade delivered by thermomechanical controlled process in GB/T 1591-2018. Q is the yield symbol, 420 is the thin-plate minimum yield in MPa, M is the delivery letter, and C is the quality letter for Charpy impact at 0°C.
The M is the point of this page. Normalized GB/T 1591 Q420NC has an N. A normalized certificate cannot be stamped MC. Grade B on the TMCP route is GB/T 1591 Q420MB. Hot-rolled GB/T 1591 Q420B has neither M nor N. Normalized D is GB/T 1591 Q420ND. Normalized E is GB/T 1591 Q420NE. The 390 MPa TMCP sister at the same temperature is GB/T 1591 Q390MC. The full family sits on GB/T 1591. Do not drop a 420 MPa drawing onto a 390 MPa plate, and do not upgrade it to GB/T 1591 Q460C without a price check.
The closest European TMCP comparison is EN 10025-4 S420M, tested at −20°C, not 0°C. EN 10025-3 S420N is normalized. On the US side, ASTM A572 Grade 60 is 60 ksi / 415 MPa, one step lower, and it is not an MC twin. ASTM A572 Gr.55 is 55 ksi. JIS G3106 SM570 is the usual Japanese comparison. Dual mark only when both books are fully met. See EN 10025-4 and high strength low alloy plates.
SHH STEEL is a global steel mill sourcing partner and steel manufacturer and exporter, mill-direct, China origin. We source Q420MC from first-line structural mills that can actually run the TMCP schedule, print heat analysis and product analysis when ordered, and ship plate to fabricators in the United States, Europe, the Middle East, Southeast Asia, Africa and South America. Related pages include structural steel plates and the products index.
Material Specification
| Specification Element | Requirement | SHH STEEL Compliance |
|---|---|---|
| Plate book | GB/T 1591-2018 Q420MC | Confirmed |
| Other search names | Q420MC steel plate, Q420 MC, Q420MC TMCP | Covered |
| Delivery condition | Thermomechanical controlled process | Confirmed |
| Yield, ≤ 16 mm | 420 MPa min | Confirmed |
| Quality grade | C, impact at 0°C | Confirmed |
| Not this page | Normalized GB/T 1591 Q420NC | Different condition |
| Warmer TMCP sister | GB/T 1591 Q420MB | +20°C |
| EN comparison | EN 10025-4 S420M is −20°C | Not a swap |
| US comparison | ASTM A572 Gr.60 is 415 MPa | Not a twin |
| Product analysis | GB/T 222 column when ordered | Confirmed |
| Supply role | Global steel mill sourcing partner | SHH STEEL |
| Certification | EN 10204 3.1 or 3.2 | As ordered |
Nearby pages that buyers compare, but must not swap blindly, include GB/T 1591 Q420NB, GB/T 1591 Q390MC and ASTM A572 Gr.55.
Chemical Composition
Heat analysis is the mill ladle table in GB/T 1591-2018 for TMCP Q420. Product analysis, when ordered, follows GB/T 222. Q420MC is a microalloyed HSLA plate. Grade C is tighter on phosphorus and sulfur than grade B, because the impact test is at 0°C. Mills may add Nb, V or Ti. The certificate shows the elements actually used. TMCP chemistry is often leaner than a normalized heat of the same yield, because the rolling schedule does part of the grain refinement.
Heat Analysis and Product Analysis — GB/T 1591 Q420MC, TMCP
| Element | Heat analysis (%) | Product analysis (%) |
|---|---|---|
| Carbon (C), max | 0.20 | 0.22 |
| Silicon (Si), max | 0.50 | 0.55 |
| Manganese (Mn), max | 1.70 | 1.80 |
| Phosphorus (P), max | 0.030 | 0.035 |
| Sulfur (S), max | 0.030 | 0.035 |
| Niobium (Nb), max | 0.07 | 0.08 |
| Vanadium (V), max | 0.20 | 0.22 |
| Titanium (Ti), max | 0.20 | 0.21 |
| Chromium (Cr), max | 0.30 | 0.35 |
| Nickel (Ni), max | 0.80 | 0.85 |
| Copper (Cu), max | 0.40 | 0.45 |
| Molybdenum (Mo), max | 0.20 | 0.21 |
| Nitrogen (N), max | 0.015 | 0.017 |
| Aluminium (Als), min when used | 0.015 | 0.010 |
Carbon equivalent is limited by thickness in the standard. The M route often has a lower CEV window than normalized GB/T 1591 Q420NC. If the purchase order writes product analysis, SHH STEEL prints both columns and the thickness band used for the tensile test. Do not treat this chemistry as quenched-and-tempered GB/T 16270 Q460C. A 390 MPa file is GB/T 1591 Q390MC, not this grade.
Mechanical Properties
Buyers search Q420MC mechanical properties, Q420MC yield strength, GB/T 1591 Q420MC tensile and Q420MC impact 0°C.
Tensile and impact — GB/T 1591 Q420MC, TMCP
| Thickness | Yield min | Tensile | Elongation min | Impact |
|---|---|---|---|---|
| ≤ 16 mm | 420 MPa | 520–680 MPa | 19% | 0°C, grade C |
| > 16–40 mm | 400 MPa | 520–680 MPa | 19% | 0°C, grade C |
| > 40–63 mm | 390 MPa | 520–680 MPa | 18% | 0°C, grade C |
| > 63–80 mm | 380 MPa | 520–680 MPa | 18% | 0°C, grade C |
| > 80–100 mm | 370 MPa | 520–680 MPa | 18% | 0°C, grade C |
| > 100–150 mm | 360 MPa | 500–660 MPa | 17% | 0°C, grade C |
Impact energy is the average of three longitudinal Charpy V-notch specimens, commonly 34 J minimum at 0°C. One value may fall below the table, but not below 70% of that value. Write a higher energy on the order if the owner requires it.
Yield steps down with thickness. A 420 MPa name on 12 mm plate is not the minimum on a 40 mm flange. 420 MPa is about 61 ksi. ASTM A572 Grade 60 is 60 ksi and is not this book. SHH STEEL quotes the thickness band and the M condition on the offer.
Density is 7.85 g/cm³. Hardness is not a design value for this grade. Z15, Z25 or Z35 through-thickness tensile is an extra, not part of the C letter.
Material Comparison
| Grade | Book | Delivery | Yield, thin plate | Impact | Swap? |
|---|---|---|---|---|---|
| GB/T 1591 Q420NC | GB/T 1591-2018 | Normalized | 420 MPa | 0°C | Different process |
| GB/T 1591 Q420MB | GB/T 1591-2018 | TMCP | 420 MPa | +20°C | Warmer M sister |
| Q420MC | GB/T 1591-2018 | TMCP | 420 MPa | 0°C | This page |
| Q420MD | GB/T 1591-2018 | TMCP | 420 MPa | −20°C | Colder M sister |
| GB/T 1591 Q390MC | GB/T 1591-2018 | TMCP | 390 MPa | 0°C | Lower yield |
| GB/T 1591 Q460C | GB/T 1591-2018 | Hot rolled | 460 MPa | 0°C | Higher yield |
| EN 10025-4 S420M | EN 10025-4 | TMCP | 420 MPa | −20°C | Colder comparison |
| ASTM A572 Gr.55 | ASTM A572 | As rolled | 380 MPa | Different | Lower yield |
A colder normalized file is GB/T 1591 Q420ND. A 355 MPa file is GB/T 1591 Q355MC.
Equivalent Material Grades
There is no official one-to-one substitute for Q420MC. What buyers compare is a 420 MPa TMCP plate tested at 0°C.
EN 10025-4 S420M is the process comparison, but it is tested at −20°C. EN 10025-3 S420N is normalized. EN 10025-2 S355JR is +20°C and only 355 MPa. In the United States, ASTM A572 Grade 60 is 60 ksi / 415 MPa. ASTM A572 Gr.55 is 55 ksi. ASTM A36 is 36 ksi and is well below this yield. In Japan, JIS G3106 SM570 is the usual comparison. SHH STEEL will not stamp EN 10025-4 S420M or ASTM A572 Gr.60 on a Q420MC certificate unless the purchase order names both books and both tables are met.
| Designation | Country / region | Standard | Notes |
|---|---|---|---|
| Q420MC | China | GB/T 1591-2018 | Name on this page |
| GB/T 1591 Q420NC | China | GB/T 1591-2018 | Normalized, not this page |
| GB/T 1591 Q420MB | China | GB/T 1591-2018 | TMCP, +20°C |
| GB/T 1591 Q390MC | China | GB/T 1591-2018 | 390 MPa, TMCP |
| EN 10025-4 S420M | Europe | EN 10025-4 | TMCP, −20°C |
| EN 10025-3 S420N | Europe | EN 10025-3 | Normalized comparison |
| ASTM A572 Gr.60 | USA | ASTM A572 | 60 ksi, lower yield |
| JIS G3106 SM570 | Japan | JIS G3106 | Usual Japanese comparison |
Structural Service
Buyers pick Q420MC when a building, bridge member or welded fabrication wants about 420 MPa yield, a TMCP condition, and impact at 0°C. Search phrases such as Q420MC steel plate and GB/T 1591 Q420MC all point here. The family index is GB/T 1591.
It is the wrong plate when the drawing says normalized. That work is GB/T 1591 Q420NC. It is the wrong plate when the drawing says hot rolled. That work is GB/T 1591 Q420B. It is the wrong plate for a +20°C file. That work is GB/T 1591 Q420MB, and the normalized sister is GB/T 1591 Q420NB. It is the wrong plate for a −20°C file. That work is Q420MD, and the normalized sister is GB/T 1591 Q420ND. It is the wrong plate for a −40°C file. That work is Q420ME, and the normalized sister is GB/T 1591 Q420NE. It is the wrong plate for a 390 MPa file. That work is GB/T 1591 Q390MC or GB/T 1591 Q390NE. It is the wrong plate for a 460 MPa file. That work is GB/T 1591 Q460NC. It is the wrong plate for a pressure vessel. That work sits on ASTM A516 or pressure vessel steel plates.
SHH STEEL supplies this plate when the drawing names GB/T 1591, quality grade C, and the M condition at 420 MPa.
Weldability
Q420MC is a weldable TMCP HSLA structural plate. Carbon is controlled, and many heats use Nb, V or Ti. A procedure written for ASTM A36 is not a finished WPS for thick Q420MC. Carbon equivalent on the M route is often lower than normalized GB/T 1591 Q420NC, which helps the root pass, but the TMCP microstructure still needs a qualified procedure. A procedure qualified only at +20°C may miss the 0°C coupon.
Typical consumables are matching 60 ksi low-hydrogen electrodes or wires. E7018-class electrodes are under-matched if the joint must develop full plate strength. A procedure written for ASTM A572 Gr.55 is a useful strength reference after chemistry is checked, but it does not cover 420 MPa. Preheat follows thickness, hydrogen and the approved WPS. Heat input should stay inside the mill window. A very high heat input can soften the TMCP zone next to the weld.
The fabricator owns the WPS. SHH STEEL can share mill heat data, product analysis and carbon equivalent for that review. Do not use a Q420MC procedure on GB/T 1591 Q355ME without checking the lower-yield carbon equivalent. Do not use it on GB/T 1591 Q460NE either.
Heat Treatment and Delivery Condition
Usual delivery from SHH STEEL for Q420MC is thermomechanical controlled process. The plate is not normalized as GB/T 1591 Q420NC and not hot rolled as GB/T 1591 Q420B.
TMCP combines controlled rolling and accelerated cooling. Finish rolling is held in the non-recrystallization range, then the plate is cooled on the run-out table to a finish temperature the mill records. Do not order Q420MC as quenched and tempered. That route belongs to GB/T 16270. Stress relief after fabrication, if used, should be agreed before cutting, because a high temper can move the TMCP properties.
The certificate lists GB/T 1591 Q420MC, heat number, delivery condition, heat analysis, product analysis when ordered, tensile by thickness band, and 0°C impact. Certificates may be EN 10204 3.1 or EN 10204 3.2. Dual marking to EN 10025-4 S420M is available only when both books are fully met.
Dimensions
Usual supply range from SHH STEEL for Q420MC steel plate:
- Thickness: commonly 8 mm – 80 mm, heavier plate to 100 mm by enquiry
- Width: 1500 mm – 3200 mm, wider by enquiry
- Length: 3000 mm – 12000 mm
Cut-to-size webs, flanges, base plates and gussets are available. Browse more sizes on structural steel plates.
Tolerances
Dimensional limits for Q420MC follow GB/T 709 unless the purchase order names EN 10029 or another table.
Typical thickness tolerance idea for Q420MC plate
| Nominal thickness (mm) | Usual minus (mm) | Usual plus (mm) |
|---|---|---|
| 8 – 15 | −0.3 | +0.8 |
| 15 – 25 | −0.4 | +0.9 |
| 25 – 40 | −0.5 | +1.1 |
| 40 – 60 | −0.6 | +1.3 |
| 60 – 80 | −0.7 | +1.5 |
| 80 – 100 | −0.8 | +1.6 |
Width on 1500–3200 mm plate is commonly held to about +20 / 0 mm or ±25 mm unless a tighter extra is named. Length on 3000–12000 mm plate is commonly held to about +50 / 0 mm. Flatness follows the agreed class. SHH STEEL will not assume a zero-minus extra on Q420MC unless the order says so.
Supplementary Requirements
Q420MC already defines 420 MPa yield, TMCP delivery and 0°C impact. Extra items still have to be written on the purchase order.
Book name. Write GB/T 1591 Q420MC. Do not write only Q420, and do not write Q420NC if the mill must stamp M. The family page is GB/T 1591.
Impact. Grade C is 0°C. Write a higher energy if the owner requires it. Do not expect a −20°C result unless the grade is changed.
Delivery condition. Write thermomechanical controlled process. Write GB/T 1591 Q420NC if normalized is required.
EN or US comparison. Write EN 10025-4 S420M or ASTM A572 Gr.60 only if dual mark is required and both tables are met. S420M is −20°C, not 0°C.
Product analysis. Write it if the file needs the second chemistry column.
Through-thickness. Z15, Z25 or Z35 when the joint is loaded through the thickness.
NDE. UT to GB/T 2970 or the named class.
Identification. Heat number, Q420MC, thickness and mill logo.
Third-party witness. EN 10204 3.2 with SGS, TÜV, BV, ABS or the inspector named.
Applications
| Industry | Typical components |
|---|---|
| Buildings and workshops | Q420MC columns, beams and base plates |
| Bridges and towers | Q420MC webs and flanges from SHH STEEL |
| Construction machinery | Q420MC frames where the drawing names M and 0°C |
| General fabrication | Q420MC gussets and connection plates |
| Comparison vs EN 10025-4 | Q420MC next to EN 10025-4 S420M |
| Comparison vs ASTM A572 | Q420MC next to ASTM A572 Gr.55 |
| Lower yield option | GB/T 1591 Q390MD when 390 MPa is enough |
Q420MC is the plate for a 420 MPa TMCP file tested at 0°C. It is the wrong plate for a painted weathering facade that needs corten. It is the wrong plate for a 690 MPa QT boom under GB/T 16270. A colder 460 MPa normalized file is GB/T 1591 Q460ND.
Supply Capability
SHH STEEL sources Q420MC from first-line Chinese structural mills and ships it on worldwide terms. Partner mills include Wuyang (Wugang), Angang, Shougang, Hanye, Anyang Iron and Steel, Baosteel, Xinyu, Xingcheng and other qualified mills when the size requires it.
Mill test certificates are issued to EN 10204 3.1 as standard. EN 10204 3.2 is arranged when the order names a third-party hold point.
Usual rolling thickness: 8 mm, 10 mm, 12 mm, 16 mm, 20 mm, 25 mm, 30 mm, 40 mm, 50 mm, 60 mm, 80 mm. Heavier plate is confirmed before order.
Processing: CNC or flame cutting, bevel, flattening, shot blast, UT to the named class.
Trade terms: FOB Shanghai main, CIF destination available. Payment: TT, LC, or TT + LC.
Ocean time from Shanghai: US West 14–18 days; US Gulf 28–35 days; Rotterdam / Antwerp 28–35 days; Jebel Ali 18–25 days; Singapore 7–12 days; other ports quoted.
Third-party: SGS, TÜV, BV, ABS, CCS, GL, VL, DNV, RINA, NK, KR, or the inspector named.
Global Delivery and Markets
SHH STEEL is a global steel mill sourcing partner with mill partnerships in China. We supply GB, ASTM, ASME, EN, DIN and JIS steel to buyers in the United States, Europe, the Middle East, Southeast Asia, Africa and South America. Origin is mill-direct, China origin.
SHH STEEL has supplied steel plates to the USA, Mexico, Argentina, Peru, El Salvador, Spain, Netherlands, Germany, UAE, Saudi Arabia, South Africa, India, Thailand, Singapore, Vietnam, the Philippines, Japan and Korea.
Typical lead time: ex-stock 5–7 days when an M heat is in yard; standard TMCP about 25–40 days; 3.2 inspection about 35–45 days.
Why Choose SHH STEEL
SHH STEEL is a global steel mill sourcing partner and steel manufacturer and exporter, mill-direct, China origin. For Q420MC that means mill-direct structural price, not a multi-layer stockist mark-up. We buy from mills that can actually run the TMCP schedule, so the M is on the certificate and not only in the enquiry.
Delivery is short when the size is in rolling range: ex-stock 5–7 days, standard M heat about 25–40 days, 3.2 inspection about 35–45 days. Cutting, bevel and UT can run in the same window. FOB Shanghai is the main term. CIF to US West, US Gulf, Rotterdam, Jebel Ali and Singapore is quoted on the same file.
Experience on this grade is simple: print GB/T 1591 Q420MC, keep the TMCP route, and do not ship GB/T 1591 Q420NC as MC. We will not drop the M to save a cooling cycle, and we will not change C to B to save a cold test. If the drawing needs normalized plate, we will move the inquiry to Q420NC. If the drawing needs 460 MPa, we will move it to GB/T 1591 Q460D or GB/T 1591 Q460NE.
FAQ
-
What is Q420MC steel plate?
- Q420MC in GB/T 1591-2018 is thermomechanical controlled process high-strength low-alloy plate with 420 MPa minimum yield on thin plate and Charpy impact at 0°C. SHH STEEL supplies this plate worldwide as a global steel mill sourcing partner.
-
Is Q420MC the same as Q420NC?
- No. Both yield at 420 MPa and both are tested at 0°C. Q420NC is normalized. Q420MC is TMCP.
-
Is Q420MC the same as Q420MB?
- No. Both are TMCP. Q420MB is tested at +20°C. Q420MC is tested at 0°C.
-
Is Q420MC the same as Q390MC?
- No. Both are TMCP and both are tested at 0°C. Q390MC is 390 MPa. Q420MC is 420 MPa.
-
What is the European equivalent of Q420MC?
- The nearest process comparison is EN 10025-4 S420M, which is TMCP but tested at −20°C. EN 10025-3 S420N is the normalized comparison. Dual mark only when both books are fully met.
-
What is the US equivalent of Q420MC?
- There is no official ASTM twin. ASTM A572 Grade 60 is 60 ksi / 415 MPa, slightly lower, and it does not carry an MC letter. SHH STEEL does not dual-mark ASTM A572 unless both books are met.
-
What thickness can SHH STEEL supply?
- Common supply is 8 mm to 80 mm. Plate to 100 mm is quoted by enquiry. Yield on plate over 16 mm is lower than the 420 MPa thin-plate number.
Conclusion
Q420MC steel plate to GB/T 1591 is 420 MPa TMCP structural plate with impact at 0°C. It is not normalized GB/T 1591 Q420NC. EN 10025-4 S420M is the TMCP comparison, tested at −20°C. ASTM A572 Grade 60 is 415 MPa and is not a substitute. Whether the inquiry says Q420MC, GB/T 1591 Q420MC or Q420MC TMCP plate, SHH STEEL as a global steel mill sourcing partner supplies plate with Q420MC chemistry, heat and product analysis as ordered, GB/T 709 tolerances and EN 10204 3.1 or 3.2 certification.
SHH STEEL supplies Q420MC Steel Plate to the United States, Europe, the Middle East, Africa, Asia and the Americas for work that actually names the M condition. The grade family is listed on GB/T 1591.
Contact SHH STEEL for mill rolling, TMCP Q420MC, cutting, UT, 3.2 inspection or a worldwide quotation.
Q420MC, Q420MC steel plate, GB/T 1591 Q420MC, Q420MC TMCP, Q420MC supplier, SHH STEEL