What is GOST 14637-2024 St3kp steel plate?
GOST 14637 St3kp Steel Plate is a rimmed (kp) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026. It was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89.
St3kp is listed in clause 6.1. The kp suffix marks a rimmed steel. It has its own Table 2 mechanical row: tensile strength 360–460 N/mm², with yield and elongation values that are not the same as the shared Table 2 row for GOST 14637 St3ps Steel Plate and GOST 14637 St3sp Steel Plate (370–480 N/mm²). In Table 1, St3kp is listed in category 1, category 2 and category 3. Category 3, which adds a KCU impact test at +20 °C, is manufactured by agreement (Table 1 footnote 6), and the +20 °C impact norms shall correspond to Table 4. St3kp is not listed in categories 4–7. A shared carbon class does not make a rimmed plate interchangeable with a semi-killed or killed St3 plate.
SHH STEEL supplies this plate in the GOST 14637 range. We review the ordered category, delivery condition and deoxidation and category before quoting production and export requirements.
Material specification for GOST 14637 St3kp
The applicable product standard for this page is GOST 14637-2024. The official English title is Rolled plates from nonalloyed steel of general quality. Specifications. Orders should state that edition, the grade St3kp, the category, dimensions, quantity and any agreed options. A grade name without an edition is incomplete. The thickness and width figures below are the standard scope, not a stock promise.
| Parameter | Detail |
|---|---|
| Standard | GOST 14637-2024; in force from 1 March 2025; replaces GOST 14637-89 |
| Official English title | Rolled plates from nonalloyed steel of general quality Specifications |
| Grade | St3kp |
| Deoxidation | Rimmed (kp), as marked by the designation suffix |
| Scope, sheets | Thickness 4 to 160 mm inclusive; width 500 mm and more |
| Scope, coils | Thickness 4 to 25 mm |
| Dimensions and tolerances | Remaining assortment requirements follow GOST 19903; state thickness accuracy and flatness on the order |
| Permitted inspection categories | 1, 2, or 3 (Table 1). Category 3 is manufactured by agreement (Table 1 footnote 6). Categories 4–7 are not listed for this grade |
| Chemical composition | Shall conform to GOST 380 (clause 7.1.1.1). Category 2 and category 3 add chemical-composition control in Table 1. A clause 7.1.1.3 option applies for thickness up to 10 mm; numeric GOST 380 limits are not tabulated on this page |
| Tensile properties | Table 2 for categories 1–5 and 7 |
| Yield strength σT | Table 2 minima, by thickness band; see Mechanical Properties |
| 180° bend | Table 5; see Mechanical Properties |
| Impact toughness | Category 3 only, by agreement: KCU at +20 °C to Table 4. Not specified in categories 1 and 2 |
| Delivery condition | Clause 7.1.6: categories 1–5 and 7 without heat treatment (hot-rolled), or thermomechanically treated, or heat-treated. Category 6 is not listed for this grade |
| Ultrasonic testing | By agreement, to a class of GOST 22727; class and volume are not implied by the grade |
| Acceptance, marking and packaging | GOST 7566, with the additions in the 2024 standard |
GOST 14637 is a general-quality nonalloyed plate standard. It is not a boiler or pressure-vessel plate standard, and it is not a quality carbon structural plate standard. Do not copy figures from those systems onto a GOST 14637 order.
Chemical composition of GOST 14637-2024 St3kp
Clause 7.1.1.1 of GOST 14637-2024 requires the chemical composition of the steel by ladle analysis of the ladle sample, and the permissible deviations in the finished product, to conform to GOST 380. This page does not tabulate GOST 380 heat-analysis limits. Confirm every chemistry cell against the applicable official GOST 380 table. This page is not a substitute for that table.
In Table 1, category 1 does not specify or control chemical composition; categories 2 and 3 do. Order category 2 or agreed category 3 when chemistry is to be a controlled characteristic. In every listed category, ladle analysis and product deviations shall conform to GOST 380.
Clause 7.1.1.2 permits manufacture without a lower limit on carbon and manganese, except for plate intended for shipbuilding, wagon-building or welded cylinders, provided the mechanical properties of this standard are met. State that option on the order if it is required.
On purchaser request, clause 7.1.1.4 tightens sulphur and phosphorus for categories 1–5 of this grade to S not more than 0.040 % and P not more than 0.030 %. For categories 6 and 7, each of these elements shall not exceed 0.025 %; those categories are not listed for this grade in Table 1. If the tighter 7.1.1.4 limits are required, state them on the order.
On purchaser request, clause 7.1.1.3 allows, for this grade at thickness up to 10 mm inclusive, a reduction of the lower limit of one of the elements of not more than 0.04 % absolute for carbon, or 0.10 % absolute for manganese, provided the mechanical properties of this standard are met. State that option on the order if it is required. This page does not tabulate the GOST 380 lower limits to which that reduction would be applied.
For subsequent hot-dip galvanizing, clause 7.1.1.5 class A (silicon not more than 0.03 %, and Si + 2.5P < 0.09 %) is the class written for rimmed (kp) steel. Classes B and D are written for killed (sp) steel and are not the class for this rimmed grade. Galvanizing class is an agreed option, not a default.
A maximum sign is an upper limit, not a target addition. Product-analysis deviations belonging to GOST 380 must not be used to widen ladle-analysis order limits. Numeric GOST 380 element ranges are not tabulated on this page.
Mechanical properties of GOST 14637-2024 St3kp
Clause 7.1.7.1 requires the tensile properties of plate in categories 1–5 and 7 to meet Table 2. The values below are from GOST 14637-2024 Table 2. Units are N/mm² for strength (the unit used in the 2024 tables) and % for elongation δ5. Table 2 heading is “not less than or within limits.”
| Property | Thickness | Requirement (Table 2) |
|---|---|---|
| Tensile strength σB, N/mm² | All thicknesses in the 2024 scope | 360–460 |
| Yield strength σT, N/mm² | ≤20 mm | ≥235 |
| Yield strength σT, N/mm² | >20 mm to 40 mm inclusive | ≥225 |
| Yield strength σT, N/mm² | >40 mm to 100 mm inclusive | ≥215 |
| Yield strength σT, N/mm² | >100 mm | ≥195 |
| Elongation δ5, % | ≤20 mm | ≥27 |
| Elongation δ5, % | >20 mm to 40 mm inclusive | ≥26 |
| Elongation δ5, % | >40 mm | ≥24 |
This is the Table 2 row that belongs to St3kp alone. It is not the shared row for GOST 14637 St3ps Steel Plate and GOST 14637 St3sp Steel Plate (370–480 N/mm², with higher yield minima and slightly lower elongation). Do not substitute those figures for this rimmed grade, and do not take yield or tensile values from another product standard.
Table 2 footnotes that apply when the corresponding cell is a specified value include the following. For coil plate of thickness over 12 mm to 25 mm inclusive, the mechanical-property norms are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. The upper tensile-strength limit may be increased by not more than 50 N/mm² while the other mechanical-property norms are observed, and by agreement with the purchaser without limiting the upper bound. By agreement, for thickness over 20 mm, the yield value may be reduced by 10 N/mm². Table 2 also permits a stated reduction of elongation for thinner plate: for thickness up to 8 mm inclusive, by 1 % absolute for each millimetre of thickness reduction; for thickness over 8 mm, by 1 % absolute. Confirm the application of this footnote against the official table when thin plate is ordered.
By agreement between the manufacturer and the purchaser, plate of St3kp, St3ps and St3sp may be supplied to Table 2 with a tensile-strength range of 370 to 550 N/mm² inclusive, in place of the grade’s own Table 2 tensile-strength cell. State that agreed range on the order if it is required.
Clause 7.1.8 requires the plate to withstand a 180° cold bend on a mandrel of the diameter in Table 5. At the bend there shall be no fracture, delamination or cracks.
| Property | Thickness (a = plate thickness) | Requirement (Table 5) |
|---|---|---|
| 180° cold bend, mandrel diameter d | ≤20 mm | d = 1.5a |
| 180° cold bend, mandrel diameter d | >20 mm to 40 mm inclusive | d = 2.5a |
| 180° cold bend, mandrel diameter d | >40 mm | d = 2.5a |
The 1.5a / 2.5a / 2.5a diameters apply to this grade except category 6; category 6 is not listed for this grade in Table 1.
Clause 7.1.7.3 requires impact tests of categories 3–7 to meet Table 4. For St3kp, only category 3 is listed, and Table 1 footnote 6 requires that category 3 be manufactured by agreement, with the +20 °C impact norms corresponding to Table 4. The Table 4 category-3 values (KCU at +20 °C, J/cm², not less than) are:
| Thickness | KCU at +20 °C, J/cm² (Table 4, category 3) |
|---|---|
| 4.0 to 10.0 mm inclusive | ≥78 |
| >10.0 to 30.0 mm inclusive | ≥69 |
| >30.0 to 40.0 mm inclusive | ≥49 |
| >40.0 to 60.0 mm inclusive | ≥49* |
| >60.0 mm | Determined for statistical data (+) |
Units are joules per square centimetre (J/cm²), not absorbed energy in joules. A plus sign means the value is determined for statistical data and is stated in the quality document; this page does not replace a plus with a number. Values marked with an asterisk are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. On one specimen, a 30 % reduction of the impact value is allowed provided the average of the test results is not below the Table 4 norm; the average is stated in the quality document. For coil plate of thickness over 12 mm to 25 mm inclusive, the impact norms are likewise optional for those two years. On purchaser request, impact work in joules may be determined instead of impact toughness, with limit values agreed between the manufacturer and the purchaser.
Impact is not a specified characteristic in categories 1 and 2 for this grade. Categories 4–7 are not listed for St3kp.
Delivery conditions for GOST 14637 St3kp
Under clause 7.1.6, plate of categories 1–5 and 7 is manufactured without heat treatment (in the hot-rolled condition), or in the thermomechanically treated or heat-treated condition. The type of thermomechanical or heat treatment, in accordance with the classification in the 2024 standard, is chosen by the manufacturer and stated in the quality document.
State the required delivery condition on the order. If the condition is omitted, do not assume a heat-treated or thermomechanically treated delivery from the grade name alone; for categories 1–5 and 7 the manufacturer may supply the plate hot-rolled. Record the actual condition on the quality document.
St3kp may be ordered in category 1, category 2, or category 3. Category 3 is manufactured by agreement (Table 1 footnote 6) and adds a KCU impact test at +20 °C to Table 4. Category 2 adds chemical-composition control without an impact test. Categories 4–7, including category 6, are not listed for this grade. A usual hot-rolled delivery is not a substitute for an agreed thermomechanical or heat-treatment condition when the project requires one.
Weldability and fabrication of GOST 14637 St3kp
On purchaser request, clause 7.1.2 allows plate to be supplied with a weldability guarantee, designated in the standard as GS. That guarantee is ensured by limiting the ladle-analysis carbon content to not more than 0.22 %. If a weldability guarantee is required, state it on the order. The designation alone does not include it.
This page does not give preheat, interpass, heat-input or post-weld heat-treatment figures. The fabricator is responsible for welding-procedure qualification, consumable selection, preheat and any post-weld heat treatment required by the project specification. Do not take those figures from another standard or from a handbook and apply them as GOST 14637 rules.
St3kp is a rimmed steel in a higher carbon class than the St2 grades. Rimmed and semi-killed or killed St3 plates are not automatic welding substitutes for each other. Do not assume that a procedure qualified on GOST 14637 St3ps Steel Plate or GOST 14637 St3sp Steel Plate, or on an St2 grade, is valid for this rimmed grade without qualification. Because official GOST 380 chemistry limits are not tabulated on this page, do not assume that ladle carbon is already at or below 0.22 %. If the weldability guarantee is required, order it and confirm the carbon restriction against the official texts.
Dimensions, surface quality and inspection
Remaining assortment requirements — dimensions, shape and permissible deviations beyond the thickness and width scope in clause 6.2.1 — follow GOST 19903. State the required thickness-accuracy class, edge condition and, for plate supplied as sheets, the flatness class on the order. This page does not tabulate numerical deviation limits from GOST 19903.
Surface quality is specified in clause 7.1.3 of the 2024 standard. Defects of the types listed there are not permitted. Dressing is allowed within the depth and area limits stated in that clause; confirm those limits against the official text. Delamination on ends and on untrimmed edges is not permitted.
Ultrasonic testing is not a default requirement. By agreement, clause 7.1.9 allows plate in sheets to be supplied with ultrasonic testing to a class of GOST 22727. The continuity class and the test volume (solid or selective) are agreed at the order; they are not implied by the grade.
Acceptance is by batch under GOST 7566, with the additions in the 2024 standard. A batch consists of sheets or coils of one steel grade, from one ladle-heat for ingot-cast product or one heat for continuously cast product. Marking and packaging follow GOST 7566. The 2024 standard allows the conventional grade number to be marked without the letters St. For destinations in the Far North and equivalent regions, packaging follows GOST 15846 when that service (HL) is stated on the order.
Applications and specification limits of St3kp
St3kp is specified where a rimmed general-quality plate, the Table 2 row for this grade (360–460 N/mm² tensile, with the stated yield and elongation), the Table 5 bend, and category 1, 2 or agreed category 3 inspection are required. Typical general-fabrication or construction use is not a design approval and is not a licence to substitute this rimmed plate for GOST 14637 St3ps Steel Plate or GOST 14637 St3sp Steel Plate, or for an St2 grade. Impact at +20 °C applies only when category 3 is ordered by agreement.
The 2024 scope is hot-rolled plate of nonalloyed steel of general quality, width 500 mm and more, thickness 4 to 160 mm inclusive (sheets) and 4 to 25 mm (coils). That is the standard scope, not a stock range. Confirm available sizes on the enquiry.
GOST 14637 is not a boiler or pressure-vessel material standard. It is not a quality carbon structural plate standard. Service temperature, toughness and forming limits are set by the project specification, not by a generic maximum-temperature claim on this page.
Compare GOST 14637 St3kp with related general-quality plates
The other general-quality designations below are in the same GOST 14637-2024 set. They are shown for a product comparison, not as equivalents. Tensile, yield and elongation figures are from Table 2 as specified in GOST 14637-2024 Table 2; the yield and elongation columns are the Table 2 values for thickness up to 20 mm inclusive. Confirm every cell, including the other thickness bands, against the official table. A similar tensile class does not authorise substitution.
| Material | Table 2 σB, N/mm² | Table 2 σT, N/mm² (≤20 mm) | Table 2 δ5, % (≤20 mm) | Relationship |
|---|---|---|---|---|
| GOST 14637 St3kp Steel Plate (this plate) | 360–460 | ≥235 | ≥27 | GOST 14637-2024; this product |
| GOST 14637 St0 Steel Plate | Not less than 300 | Not specified | ≥23 | 2024 edition; related, not interchangeable |
| GOST 14637 St2kp Steel Plate | 320–410 | ≥215 | ≥33 | 2024 edition; different carbon class; related, not interchangeable |
| GOST 14637 St2ps Steel Plate | 330–430 | ≥225 | ≥32 | 2024 edition; different carbon class; related, not interchangeable |
| GOST 14637 St2sp Steel Plate | 330–430 | ≥225 | ≥32 | 2024 edition; different carbon class; related, not interchangeable |
| GOST 14637 St3ps Steel Plate | 370–480 | ≥245 | ≥26 | 2024 edition; different Table 2 row and deoxidation; related, not interchangeable |
| GOST 14637 St3sp Steel Plate | 370–480 | ≥245 | ≥26 | 2024 edition; different Table 2 row and deoxidation; related, not interchangeable |
St3kp is the rimmed grade in this carbon class and has its own Table 2 row. GOST 14637 St3ps Steel Plate and GOST 14637 St3sp Steel Plate share a different row (370–480 N/mm²). The St2 grades are a lower carbon class. None of these is a substitute for this rimmed plate.
GB/T 700 ordinary carbon structural steel is a different standard with a different chemistry and property system. St3kp is commonly compared with GB/T 700 Q235B, EN 10025-2 S235JR and JIS G3101 SS400; that comparison is not equivalence. Related ordinary structural plate systems, including EN 10025-2, JIS G3101 and ASTM A283, are sometimes listed on comparison charts. A chart cannot replace a review of chemistry, deoxidation, category, mechanical tests and the project specification.
Equivalent material grades for GOST 14637 St3kp
No formal equivalence has been verified for the designations below. They are related designations only and are not equivalent to this GOST 14637-2024 plate. Engineer approval is required before any substitution. This page does not link any external catalogue.
| Standard | Country-Region | Equivalent Grade | Note |
|---|---|---|---|
| GOST 14637-2024 | Interstate (GOST) | St3kp | This product under GOST 14637-2024, category 1, category 2, or category 3 (category 3 by agreement). Rimmed (kp) deoxidation; own Table 2 row. Category 3 is by agreement. |
| GB/T 700 | China | GB/T 700 Q235B | Commonly compared; not equivalent. Verify chemistry, mechanicals, deoxidation, inspection category and the project specification. A similar tensile class does not authorise substitution. Engineer approval is required. Not a verified formal equivalent. |
| EN 10025-2 | Europe | EN 10025-2 S235JR | Commonly compared; not equivalent. Verify chemistry, mechanicals, deoxidation, inspection category and the project specification. A similar tensile class does not authorise substitution. Engineer approval is required. Not a verified formal equivalent. |
| JIS G3101 | Japan | JIS G3101 SS400 | Commonly compared; not equivalent. Verify chemistry, mechanicals, deoxidation, inspection category and the project specification. A similar tensile class does not authorise substitution. Engineer approval is required. Not a verified formal equivalent. |
Related ordinary structural plate systems, including EN 10025-2, JIS G3101 and ASTM A283, are sometimes listed on comparison charts. No additional specific grade in those systems is listed as a verified equivalent on this page beyond the commonly compared designations in the table above. A chart cannot replace a review of chemistry, product form, delivery condition, mechanical tests and the project specification.
Within this site, compare the present plate with GOST 14637 St0 Steel Plate, GOST 14637 St2kp Steel Plate, GOST 14637 St2ps Steel Plate, GOST 14637 St2sp Steel Plate, GOST 14637 St3kp Steel Plate, GOST 14637 St3ps Steel Plate, GOST 14637 St3sp Steel Plate in the GOST 14637 range, and with the different structural system under GB/T 700.
Why choose SHH STEEL for GOST 14637 St3kp
- SHH STEEL produces and exports St3kp rimmed general-quality plate to the ordered GOST 14637-2024 specification
- We quote against the 2024 edition that is in force, and we use the Table 2 row that belongs to this rimmed grade, not the shared St3ps / St3sp row
- Category (1, 2, or agreed category 3 with Table 4 KCU at +20 °C), deoxidation and any agreed chemistry or weldability options are written on the quotation
- The quotation states thickness, width, delivery condition, any agreed ultrasonic test, and the inspection document — not a generic stock grade alone
- We review cutting, packaging, traceability and export documentation before confirming the order
How to enquire for GOST 14637 St3kp plate
Send the drawing or material schedule with the following details. Production feasibility, dimensions, documentation and delivery are confirmed against the enquiry.
| Item | What to specify |
|---|---|
| Edition and grade | GOST 14637-2024 St3kp (rimmed, kp); do not assume the withdrawn 1989 edition, a different deoxidation, or dual certification |
| Category | Category 1, 2, or 3 (category 3 by agreement, with Table 4 KCU at +20 °C) |
| Dimensions and quantity | Thickness, width, length and tonnage, within the 2024 scope of 4–160 mm for sheets (4–25 mm for coils) and width 500 mm and more |
| Product form | Sheets or coils, as applicable |
| Delivery condition | Hot-rolled without heat treatment, or a stated thermomechanical or heat-treatment condition; record the actual condition on the quality document |
| Chemistry options | GOST 380 conformity; clause 7.1.1.3 lower-limit reduction for thickness ≤10 mm if required; tighter S and P under clause 7.1.1.4 if required; galvanizing class A if required |
| Agreed tensile range | If required: 370–550 N/mm² inclusive, in place of the Table 2 360–460 N/mm² cell |
| Weldability guarantee | If required: GS, ladle carbon not more than 0.22 %; not implied by the grade |
| Ultrasonic examination | GOST 22727 class and volume as ordered; not implied by the grade |
| Surface and tolerances | GOST 19903 thickness accuracy, edge condition and flatness class as ordered |
| Documentation | Quality-document requirements under GOST 7566, heat traceability, and any third-party inspection |
FAQ
-
Is GOST 14637-2024 current for St3kp?
- Yes. GOST 14637-2024 is the current edition as of 12 November 2026. It was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89. State the 2024 edition, the grade St3kp, the category (1, 2, or agreed 3) and the rimmed (kp) deoxidation on the order. Do not use 1989 tables for a 2024 order.
-
What thickness and width does GOST 14637-2024 specify for St3kp?
- The 2024 scope is thickness 4 to 160 mm inclusive for sheets and 4 to 25 mm for coils, with width 500 mm and more. That is the standard scope, not a stock range. Confirm available sizes on the enquiry. Remaining dimensional requirements follow GOST 19903.
-
How does St3kp differ from St3ps and St3sp?
- St3kp is rimmed (kp) and has its own Table 2 row: tensile strength 360–460 N/mm², yield ≥235 / ≥225 / ≥215 / ≥195 N/mm² and elongation δ5 ≥27 / ≥26 / ≥24 % in the stated thickness bands. St3ps (semi-killed) and St3sp (killed) share a different Table 2 row (370–480 N/mm²). St3kp is listed in categories 1–3 only (category 3 by agreement, with Table 4 KCU at +20 °C); it is not listed in categories 4–7. A shared carbon class is not interchangeability.
-
What inspection categories apply to St3kp, and does it have an impact test?
- Table 1 lists St3kp in category 1, category 2 and category 3. Categories 1 and 2 specify tensile properties and a 180° bend; category 2 adds chemistry control. Category 3 is manufactured by agreement and adds a KCU impact test at +20 °C to Table 4 (78 / 69 / 49 / 49* / statistical, in J/cm², by thickness band). Categories 4–7 are not listed for this grade. State the category on the order.
-
Is GOST 14637 St3kp equivalent to GB/T 700 Q235B or EN 10025-2 S235JR?
- No. St3kp is commonly compared with GB/T 700 Q235B, EN 10025-2 S235JR and JIS G3101 SS400; those comparisons are not equivalence. The products belong to different standards, with different chemistry rules, mechanical tables, deoxidation practice and inspection categories. Engineer approval is required before any substitution. Send the design requirements with the enquiry; we do not assume interchangeability.
Request a quotation for GOST 14637 St3kp plate
Contact SHH STEEL for a quotation for GOST 14637-2024 St3kp rimmed general-quality steel plate. Send thickness, width, length, quantity, destination and the project material specification.
Specify the 2024 edition, the rimmed (kp) grade St3kp, the category (1, 2, or agreed 3), the product form, the delivery condition, any agreed chemistry option, ultrasonic test or weldability guarantee, and the quality-document requirement. Do not assume a semi-killed or killed deoxidation, categories 4–7, or the withdrawn 1989 edition.
If a related grade or another standard is being considered, send the design requirements for review. We do not assume interchangeability from a grade comparison alone.