GOST 14637 St3sp Steel Plate | St3sp Killed Carbon Steel Plate | GOST 14637 Steel - SHH STEEL

GOST 14637 St3sp Steel Plate | St3sp Killed Carbon Steel Plate

GOST 14637 St3sp (Ст3сп) steel plate is a killed (sp) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026: it was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89. SHH STEEL produces and exports this killed grade to the ordered 2024 requirements.
Grade
St3sp
Standard
GOST 14637-2024
Deoxidation
Killed (sp)
Categories (Table 1)
1–7
Tensile strength (Table 2)
370–480 N/mm²
Delivery (clause 7.1.6)
Cats 1–5 & 7: HR, TM or HT; cat 6: TM or HT only
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

General Description of GOST 14637 St3sp Steel Plate

GOST 14637 St3sp Steel Plate is a killed (sp) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026. It was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89.

St3sp is listed in clause 6.1. The sp suffix marks a killed steel. In Table 2, St3sp shares one mechanical row with GOST 14637 St3ps Steel Plate (tensile strength 370–480 N/mm²). A shared row is not interchangeability: St3sp is killed and St3ps is semi-killed. GOST 14637 St3Gps Steel Plate has its own tensile-strength cell (370–490 N/mm²) with the same yield and elongation as that shared row. GOST 14637 St3Gsp Steel Plate has a different Table 2 row (390–570 N/mm², with statistical (+) cells in the thicker yield and elongation bands). GOST 14637 St3kp Steel Plate is the rimmed grade in the same carbon class and has a different Table 2 row (360–460 N/mm²). In Table 1, St3sp is listed in categories 1–7, including the impact categories 3–7 and category 6, whose tensile properties follow Table 3 and whose 180° bend follows a different Table 5 row. State the category on the order.

SHH STEEL supplies this plate in the GOST 14637 range. We review the ordered category, delivery condition and deoxidation and category before quoting production and export requirements.

GOST 14637 St3sp Steel Plate Material Specification

The applicable product standard for this page is GOST 14637-2024. The official English title is Rolled plates from nonalloyed steel of general quality. Specifications. Orders should state that edition, the grade St3sp, the category, dimensions, quantity and any agreed options. A grade name without an edition is incomplete. The thickness and width figures below are the standard scope, not a stock promise.

Parameter Detail
Standard GOST 14637-2024; in force from 1 March 2025; replaces GOST 14637-89
Official English title Rolled plates from nonalloyed steel of general quality Specifications
Grade St3sp
Deoxidation Killed (sp), as marked by the designation suffix
Scope, sheets Thickness 4 to 160 mm inclusive; width 500 mm and more
Scope, coils Thickness 4 to 25 mm
Dimensions and tolerances Remaining assortment requirements follow GOST 19903; state thickness accuracy and flatness on the order
Permitted inspection categories 1–7 (Table 1). Category 6 uses Table 3 tensile properties and a different Table 5 bend row, and is delivered thermomechanically treated or heat-treated
Chemical composition Shall conform to GOST 380 (clause 7.1.1.1). Categories 2–7 add chemical-composition control in Table 1. A clause 7.1.1.3 option applies for thickness up to 10 mm; numeric GOST 380 limits are not tabulated on this page
Tensile properties Table 2 for categories 1–5 and 7; Table 3 for category 6
Yield strength σT Table 2 minima for categories 1–5 and 7, in the row shared with St3ps; Table 3 minima for category 6. See Mechanical Properties
180° bend Table 5; see Mechanical Properties
Impact toughness Categories 3–7: Table 4, in J/cm². Not specified in categories 1 and 2
Delivery condition Clause 7.1.6: categories 1–5 and 7 without heat treatment (hot-rolled), or thermomechanically treated, or heat-treated; category 6 thermomechanically treated or heat-treated only
Ultrasonic testing By agreement, to a class of GOST 22727; class and volume are not implied by the grade
Acceptance, marking and packaging GOST 7566, with the additions in the 2024 standard

GOST 14637 is a general-quality nonalloyed plate standard. It is not a boiler or pressure-vessel plate standard, and it is not a quality carbon structural plate standard. Do not copy figures from those systems onto a GOST 14637 order.

GOST 14637 St3sp Steel Plate Chemical Composition

Clause 7.1.1.1 of GOST 14637-2024 requires the chemical composition of the steel by ladle analysis of the ladle sample, and the permissible deviations in the finished product, to conform to GOST 380. This page does not tabulate GOST 380 heat-analysis limits. Confirm every chemistry cell against the applicable official GOST 380 table. This page is not a substitute for that table.

In Table 1, category 1 does not specify or control chemical composition; categories 2–7 do. Order a category from 2 upwards when chemistry is to be a controlled characteristic. In every listed category, ladle analysis and product deviations shall conform to GOST 380.

Clause 7.1.1.2 permits manufacture without a lower limit on carbon and manganese, except for plate intended for shipbuilding, wagon-building or welded cylinders, provided the mechanical properties of this standard are met. State that option on the order if it is required.

On purchaser request, clause 7.1.1.4 tightens sulphur and phosphorus for categories 1–5 of this grade to S not more than 0.040 % and P not more than 0.030 %. For categories 6 and 7, each of these elements shall not exceed 0.025 %; those categories are listed for St3sp and apply when they are ordered. If the tighter 7.1.1.4 limits are required for categories 1–5, state them on the order.

On purchaser request, clause 7.1.1.3 allows, for this grade at thickness up to 10 mm inclusive, a reduction of the lower limit of one of the elements of not more than 0.04 % absolute for carbon, or 0.10 % absolute for manganese, provided the mechanical properties of this standard are met. State that option on the order if it is required. This page does not tabulate the GOST 380 lower limits to which that reduction would be applied.

For subsequent hot-dip galvanizing, clause 7.1.1.5 allows agreed silicon classes. Classes B (silicon 0.14 % to 0.25 %) and D (silicon 0.25 % to 0.35 %) are the classes written for killed (sp) steel. Class A is written for rimmed (kp) steel and is not the class for this killed grade. Galvanizing class is an agreed option, not a default.

A maximum sign is an upper limit, not a target addition. Product-analysis deviations belonging to GOST 380 must not be used to widen ladle-analysis order limits. Numeric GOST 380 element ranges are not tabulated on this page.

GOST 14637 St3sp Steel Plate Mechanical Properties

Clause 7.1.7.1 requires the tensile properties of plate in categories 1–5 and 7 to meet Table 2. The values below are from GOST 14637-2024 Table 2. Units are N/mm² for strength (the unit used in the 2024 tables) and % for elongation δ5. Table 2 heading is “not less than or within limits.”

Property Thickness Requirement (Table 2)
Tensile strength σB, N/mm² All thicknesses in the 2024 scope 370–480
Yield strength σT, N/mm² ≤20 mm ≥245
Yield strength σT, N/mm² >20 mm to 40 mm inclusive ≥235
Yield strength σT, N/mm² >40 mm to 100 mm inclusive ≥225
Yield strength σT, N/mm² >100 mm ≥205
Elongation δ5, % ≤20 mm ≥26
Elongation δ5, % >20 mm to 40 mm inclusive ≥25
Elongation δ5, % >40 mm ≥23

This Table 2 row is shared by St3sp and GOST 14637 St3ps Steel Plate (tensile strength 370–480 N/mm²). A shared row is not interchangeability: the two grades differ by deoxidation (killed against semi-killed). GOST 14637 St3Gps Steel Plate has a wider tensile-strength cell (370–490 N/mm²) with the same yield and elongation as this shared row. GOST 14637 St3Gsp Steel Plate has a different Table 2 row (390–570 N/mm², with statistical (+) cells in the thicker bands). GOST 14637 St3kp Steel Plate has a different Table 2 row (360–460 N/mm², with lower yield minima and higher elongation). Do not take figures from those other rows, and do not take yield or tensile values from another product standard.

Table 2 footnotes that apply when the corresponding cell is a specified value include the following. For coil plate of thickness over 12 mm to 25 mm inclusive, the mechanical-property norms are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. The upper tensile-strength limit may be increased by not more than 50 N/mm² while the other mechanical-property norms are observed, and by agreement with the purchaser without limiting the upper bound. By agreement, for thickness over 20 mm, the yield value may be reduced by 10 N/mm². Table 2 also permits a stated reduction of elongation for thinner plate: for thickness up to 8 mm inclusive, by 1 % absolute for each millimetre of thickness reduction; for thickness over 8 mm, by 1 % absolute. Confirm the application of this footnote against the official table when thin plate is ordered.

By agreement between the manufacturer and the purchaser, plate of St3kp, St3ps and St3sp may be supplied to Table 2 with a tensile-strength range of 370 to 550 N/mm² inclusive, in place of the grade’s own Table 2 tensile-strength cell (370–480 N/mm²). State that agreed range on the order if it is required.

For category 6 only, clause 7.1.7.2 requires tensile properties to meet Table 3, not Table 2. Table 3 is not grade-specific. Values are minima:

Thickness Tensile strength σB, N/mm² Yield strength σT, N/mm² Elongation δ5, %
Up to 40 mm inclusive ≥430 ≥295 ≥16
>40 mm Determined for statistical data (+) Determined for statistical data (+) Determined for statistical data (+)

A plus sign in Table 3 means the characteristic is determined for statistical data and is stated in the quality document. The same two-year optional-norm footnote for coil plate of thickness over 12 mm to 25 mm inclusive applies. Category 6 is delivered in the thermomechanically treated or heat-treated condition (clause 7.1.6).

Clause 7.1.8 requires the plate to withstand a 180° cold bend on a mandrel of the diameter in Table 5. At the bend there shall be no fracture, delamination or cracks. The 1.5a / 2.5a / 2.5a diameters apply except when category 6 is ordered:

Property Thickness (a = plate thickness) Requirement (Table 5)
180° cold bend, mandrel diameter d ≤20 mm d = 1.5a
180° cold bend, mandrel diameter d >20 mm to 40 mm inclusive d = 2.5a
180° cold bend, mandrel diameter d >40 mm d = 2.5a

For category 6 of St3ps, St3sp, St3Gps and St3Gsp, Table 5 prescribes larger mandrel diameters. Those diameters apply only when category 6 is ordered:

Property (category 6) Thickness (a = plate thickness) Requirement (Table 5)
180° cold bend, mandrel diameter d ≤20 mm d = 4a
180° cold bend, mandrel diameter d >20 mm to 40 mm inclusive d = 5a
180° cold bend, mandrel diameter d >40 mm d = 5a*

The asterisk on d = 5a for thickness over 40 mm in the category-6 row means the 180° bend result is optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document.

Clause 7.1.7.3 requires impact tests of categories 3–7 to meet Table 4. St3sp is listed in all of those categories, and also in categories 1 and 2, where impact is not a specified characteristic. Table 4 gives values “in accordance with Table 1”; the figures below are the Table 4 cells for categories 3–7. Units are J/cm², not less than.

Category 3 (KCU at +20 °C), J/cm², not less than:

Thickness KCU at +20 °C, J/cm² (Table 4, category 3)
4.0 to 10.0 mm inclusive ≥78
>10.0 to 30.0 mm inclusive ≥69
>30.0 to 40.0 mm inclusive ≥49
>40.0 to 60.0 mm inclusive ≥49*
>60.0 mm Determined for statistical data (+)

Category 4 (KCU at −20 °C), J/cm², not less than:

Thickness KCU at −20 °C, J/cm²
4.0 to 10.0 mm inclusive ≥39
>10.0 to 30.0 mm inclusive ≥29
>30.0 to 40.0 mm inclusive ≥29*
>40.0 to 60.0 mm inclusive ≥29*
>60.0 mm Determined for statistical data (+)

Category 5 (KCU at −20 °C, KCU after mechanical aging, and KCV at +20 °C), J/cm², not less than:

Thickness KCU at −20 °C KCU after mechanical aging KCV at +20 °C
4.0 to 10.0 mm inclusive ≥39 ≥39 ≥34
>10.0 to 20.0 mm inclusive ≥29 ≥29 ≥34
>20.0 to 30.0 mm inclusive ≥29 ≥29 ≥34*
>30.0 to 40.0 mm inclusive ≥29* ≥29 ≥34*
>40.0 to 60.0 mm inclusive ≥29* ≥29* ≥29*
>60.0 mm + + +

Category 6 (KCU at −40 °C, KCU after mechanical aging, and KCV at 0 °C), J/cm², not less than:

Thickness KCU at −40 °C KCU after mechanical aging KCV at 0 °C
4.0 to 10.0 mm inclusive ≥39 ≥39 ≥34
>10.0 to 20.0 mm inclusive ≥39 ≥29 ≥30
>20.0 to 40.0 mm inclusive ≥39 ≥29 ≥29*
>40.0 to 60.0 mm inclusive ≥39* ≥29* ≥29*
>60.0 mm + + +

Category 7 (KCU at −40 °C, KCU after mechanical aging, and KCV at −20 °C), J/cm², not less than:

Thickness KCU at −40 °C KCU after mechanical aging KCV at −20 °C
4.0 to 10.0 mm inclusive ≥39 ≥29 ≥34*
>10.0 to 40.0 mm inclusive ≥39 ≥29 ≥34*
>40.0 to 60.0 mm inclusive ≥39* ≥29* ≥29*
>60.0 mm + + +

Units are joules per square centimetre (J/cm²), not absorbed energy in joules. A plus sign means the value is determined for statistical data and is stated in the quality document; this page does not replace a plus with a number. Values marked with an asterisk are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. On one specimen, a 30 % reduction of the impact value is allowed provided the average of the test results is not below the Table 4 norm; the average is stated in the quality document. For coil plate of thickness over 12 mm to 25 mm inclusive, the impact norms are likewise optional for those two years. On purchaser request, impact work in joules may be determined instead of impact toughness, with limit values agreed between the manufacturer and the purchaser.

For categories 2 and 3 of St3ps and St3sp at thickness 5 mm and more (except plate intended for tubes), Table 1 footnote 4 states that manufacture is by agreement between the manufacturer and the purchaser; confirm the full wording of that footnote against the official table. For category 5 plate intended for tubes, Table 1 has a further footnote on additional impact tests to be stated in the order; confirm the full wording of that footnote against the official table.

GOST 14637 St3sp Steel Plate Delivery Conditions

Under clause 7.1.6, plate of categories 1–5 and 7 is manufactured without heat treatment (in the hot-rolled condition), or in the thermomechanically treated condition, or in the heat-treated condition. Category 6 is manufactured in the thermomechanically treated or heat-treated condition only. State the required delivery condition on the order. If the condition is omitted, do not assume a heat-treated or thermomechanically treated delivery from the grade name alone; for the categories in the 1–5 and 7 group that are listed for this grade, the manufacturer may supply the plate hot-rolled. Record the actual condition on the quality document.

St3sp may be ordered in any of categories 1–7. State the category on the order. Category 6 is manufactured in the thermomechanically treated or heat-treated condition only, and its tensile properties follow Table 3 rather than Table 2. Categories 3–7 add the Table 4 impact tests. For categories 2 and 3 at thickness 5 mm and more (except plate intended for tubes), Table 1 footnote 4 requires manufacture by agreement; confirm the full wording of that footnote against the official table.

GOST 14637 St3sp Steel Plate Weldability

On purchaser request, clause 7.1.2 allows plate to be supplied with a weldability guarantee, designated in the standard as GS. That guarantee is ensured by limiting the ladle-analysis carbon content to not more than 0.22 %. If a weldability guarantee is required, state it on the order. The designation alone does not include it.

This page does not give preheat, interpass, heat-input or post-weld heat-treatment figures. The fabricator is responsible for welding-procedure qualification, consumable selection, preheat and any post-weld heat treatment required by the project specification. Do not take those figures from another standard or from a handbook and apply them as GOST 14637 rules.

St3sp is a killed steel in the St3 class. Killed, semi-killed and rimmed St3 plates, and the manganese (G) St3 grades GOST 14637 St3Gps Steel Plate and GOST 14637 St3Gsp Steel Plate, are not automatic welding substitutes for each other. Do not assume that a procedure qualified on GOST 14637 St3ps Steel Plate, GOST 14637 St3kp Steel Plate, or a manganese St3 grade is valid for this killed grade without qualification. Because official GOST 380 chemistry limits are not tabulated on this page, do not assume that ladle carbon is already at or below 0.22 %. If the weldability guarantee is required, order it and confirm the carbon restriction against the official texts.

GOST 14637 St3sp Steel Plate Tolerances

Remaining assortment requirements — dimensions, shape and permissible deviations beyond the thickness and width scope in clause 6.2.1 — follow GOST 19903. State the required thickness-accuracy class, edge condition and, for plate supplied as sheets, the flatness class on the order. This page does not tabulate numerical deviation limits from GOST 19903.

Surface quality is specified in clause 7.1.3 of the 2024 standard. Defects of the types listed there are not permitted. Dressing is allowed within the depth and area limits stated in that clause; confirm those limits against the official text. Delamination on ends and on untrimmed edges is not permitted.

Ultrasonic testing is not a default requirement. By agreement, clause 7.1.9 allows plate in sheets to be supplied with ultrasonic testing to a class of GOST 22727. The continuity class and the test volume are not implied by the grade or the category; state them on the order if they are required.

GOST 14637 St3sp Steel Plate Applications and service limits

GOST 14637-2024 is a general-quality nonalloyed plate specification. Typical uses are structural and general fabrication where the ordered category, thickness and delivery condition of this grade meet the project specification. This page does not assign a service temperature, a pressure rating or a code-allowed stress from the grade name. The purchaser and the designer remain responsible for fitness for the intended duty.

St3sp is the killed St3 grade and may be ordered across categories 1–7, including the impact categories 3–7 and the thermomechanically treated or heat-treated category 6. A killed deoxidation does not by itself qualify the plate for a low-temperature or pressure duty. Select the category that matches the required impact test, and do not treat a category-1 or category-2 plate as a substitute for a Table 4 impact order. For a different product family, see the ASTM A283/A283M hub. This grade is not a boiler or pressure-vessel plate and is not a quality carbon structural plate; do not copy figures from those systems onto the order.

Compare St3sp with related GOST 14637 grades

The figures in the table below are from GOST 14637-2024 Table 2 (and the Table 1 category lists). They compare grades inside this standard. A shared carbon class, a shared yield cell or a nearby tensile-strength range is not interchangeability.

Grade Table 2 tensile σB, N/mm² Yield σT, ≤20 mm Elongation δ5, ≤20 mm Table 1 categories
GOST 14637 St3kp Steel Plate 360–460 ≥235 ≥27 1–3
GOST 14637 St3ps Steel Plate 370–480 ≥245 ≥26 1–7
GOST 14637 St3sp Steel Plate (this page) 370–480 ≥245 ≥26 1–7
GOST 14637 St3Gps Steel Plate 370–490 ≥245 ≥26 3–7
GOST 14637 St3Gsp Steel Plate 390–570 ≥255 ≥23 3–7

St3sp shares its full Table 2 row with GOST 14637 St3ps Steel Plate. The difference is deoxidation: this page is the killed grade. GOST 14637 St3Gps Steel Plate uses the same yield and elongation cells but a wider tensile-strength cell (370–490 N/mm²) and is listed only in categories 3–7. GOST 14637 St3Gsp Steel Plate has a higher tensile-strength cell (390–570 N/mm²) and statistical (+) yield and elongation in the thicker bands. GOST 14637 St3kp Steel Plate is the rimmed St3 grade, with a lower tensile-strength cell and listing only through category 3. None of those relationships is interchangeability.

Purchasers commonly compare the St3 class with GB/T 700 Q235B, EN 10025-2 S235JR and JIS G3101 SS400. A common comparison is not an equivalent. Those grades belong to other product standards, with their own chemistry, tensile, impact and delivery rules. See also the GB/T 700 hub, the EN 10025-2 hub and the JIS G3101 hub. Do not copy a yield, impact or chemistry figure from those pages onto a GOST 14637 order.

GOST 14637 St3sp Steel Plate Equivalent Material Grade

The entries below are commonly compared designations, not equivalent grades. GOST 14637-2024 does not publish a one-to-one equivalent-grade table for this designation. A comparable tensile class in another standard is not a substitute: chemistry, deoxidation, impact category and delivery condition must each be checked against the official texts.

Standard Country-Region Equivalent Grade Note
GB/T 700 China GB/T 700 Q235B Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.
EN 10025-2 Europe EN 10025-2 S235JR Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.
JIS G3101 Japan JIS G3101 SS400 Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.

If a project specification names one of those other grades, order that specification. If it names St3sp under GOST 14637-2024, order this grade and the required category. Do not treat a cross-reference as a certified equivalent.

Why choose Us

SHH STEEL produces and exports GOST 14637 plate, including St3sp. We review the killed deoxidation, the Table 2 row shared with St3ps, the agreed 370–550 N/mm² tensile option, and the category — including category 6 and the Table 4 impact categories before production, and we state the actual results on the quality document. We do not treat a shared Table 2 cell or a commonly compared foreign grade as a substitute for the ordered designation.

Orders are accepted against GOST 14637-2024. Enquiry details should include grade, category, thickness, width, length or coil mass, quantity, delivery condition and any agreed options (weldability guarantee, galvanizing class, tighter sulphur and phosphorus, ultrasonic class). See the GOST 14637 hub for the product family.

Our Service

Supply covers production to the ordered 2024 requirements, mill documentation, and export packing and shipment. Quality documents record the actual ladle analysis, tensile results and, where the category requires them, impact results, including any characteristic that Table 2, Table 3 or Table 4 marks as determined for statistical data. Ultrasonic testing, a weldability guarantee and a galvanizing class are supplied when they are agreed on the order, not by default.

To enquire, state GOST 14637-2024, grade St3sp, the Table 1 category, dimensions, quantity and the required options. SHH STEEL will confirm manufacturability and the inspection plan against that order. This page is a product description; the official standard and the quality document govern acceptance.

FAQ

What is GOST 14637 St3sp steel plate?

St3sp (Ст3сп) is the killed (sp) St3 grade under GOST 14637-2024. In Table 2 it shares a mechanical row with GOST 14637 St3ps Steel Plate (tensile strength 370–480 N/mm²). A shared row is not interchangeability. It is listed in Table 1 categories 1–7, including the impact categories 3–7 and category 6.

Which inspection categories apply to St3sp?

Table 1 lists St3sp in categories 1–7. Category 1 does not control chemical composition or impact. Categories 2–7 control chemistry. Categories 3–7 add Table 4 impact tests. Category 6 uses Table 3 tensile properties, a different Table 5 bend row, and a thermomechanically treated or heat-treated delivery only. For categories 2 and 3 at thickness 5 mm and more (except tube plate), manufacture is by agreement (Table 1 footnote 4); confirm that footnote against the official table. State the category on the order.

What are the Table 2 tensile properties of St3sp?

Tensile strength is 370–480 N/mm². Yield minima are 245, 235, 225 and 205 N/mm² in the four thickness bands. Elongation δ5 minima are 26, 25 and 23 %. By agreement, St3kp, St3ps and St3sp may be supplied to Table 2 with a tensile-strength range of 370 to 550 N/mm² inclusive. For category 6, tensile properties follow Table 3, not Table 2.

Is St3sp interchangeable with St3ps, St3Gps or St3Gsp?

No. GOST 14637 St3ps Steel Plate shares this Table 2 row but is semi-killed. GOST 14637 St3Gps Steel Plate has a wider tensile-strength cell (370–490 N/mm²) and is listed only in categories 3–7. GOST 14637 St3Gsp Steel Plate has a different Table 2 row (390–570 N/mm², with statistical (+) cells in the thicker bands). A shared row, a shared St3 class or a nearby tensile range is not interchangeability. GOST 14637 St3kp Steel Plate is the rimmed St3 grade, with its own row.

Where is the chemical composition of St3sp specified?

Clause 7.1.1.1 requires ladle analysis and product deviations to conform to GOST 380. This page does not tabulate those GOST 380 cells. Confirm them against the applicable official GOST 380 table. Category 2 upwards adds chemistry control in Table 1 of GOST 14637-2024. Clause 7.1.1.3 (a stated lower-limit reduction at thickness up to 10 mm) is written for this grade. Tighter sulphur and phosphorus follow clause 7.1.1.4 when requested or when categories 6 and 7 are ordered.

Enquire about GOST 14637 St3sp Steel Plate

Enquire for GOST 14637 St3sp Steel Plate to GOST 14637-2024. State the category (1–7), thickness, width, length or coil mass, quantity, delivery condition and any agreed options. SHH STEEL will review the killed deoxidation, the Table 2 row (370–480 N/mm²) and the required impact category before quoting production and export.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X