GOST 14637 St4sp (Ст4сп) steel plate is a killed (sp) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026: it was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89. SHH STEEL produces and exports this killed grade to the ordered 2024 requirements.
Grade
St4sp
Standard
GOST 14637-2024
Deoxidation
Killed (sp)
Categories (Table 1)
3 only (not 1–2 or 4–7)
Tensile strength (Table 2)
410–530 N/mm²
180° bend (Table 5)
d = 2.5a / 3.5a / 3.5a
Delivery (clause 7.1.6)
Cat 3: HR, TM or HT (cat 6 not listed)
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

General Description of GOST 14637 St4sp Steel Plate

GOST 14637 St4sp Steel Plate is a killed (sp) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026. It was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89.

St4sp is listed in clause 6.1. In Table 2, St4sp shares one mechanical row with GOST 14637 St4ps Steel Plate (tensile strength 410–530 N/mm²). A shared row is not interchangeability: St4sp is killed (sp), killed and St4ps is semi-killed. The 1989 rimmed grade Ст4кп (St4kp) is not listed in clause 6.1 or in Table 1 of the 2024 edition and is not a 2024 supply grade. In Table 1, St4sp is listed in category 3 only. Categories 1, 2 and 4–7 are not listed, so every listed supply includes chemical-composition control and a KCU impact test at +20 °C to Table 4. GOST 14637 St5ps Steel Plate and GOST 14637 St5sp Steel Plate have a higher Table 2 tensile-strength cell (490–630 N/mm²) and are listed only in categories 1 and 2, where impact is not specified. GOST 14637 St3sp Steel Plate is listed in categories 1–7, with a lower tensile-strength cell (370–480 N/mm²). A nearby tensile class is not interchangeability. State the category on the order.

SHH STEEL supplies this plate in the GOST 14637 range. We review the ordered category, delivery condition and deoxidation and the category-3 listing before quoting production and export requirements.

GOST 14637 St4sp Steel Plate Material Specification

The applicable product standard for this page is GOST 14637-2024. The official English title is Rolled plates from nonalloyed steel of general quality. Specifications. Orders should state that edition, the grade St4sp, the category, dimensions, quantity and any agreed options. A grade name without an edition is incomplete. The thickness and width figures below are the standard scope, not a stock promise.

Parameter Detail
Standard GOST 14637-2024; in force from 1 March 2025; replaces GOST 14637-89
Official English title Rolled plates from nonalloyed steel of general quality Specifications
Grade St4sp
Deoxidation Killed (sp), as marked by the designation
Scope, sheets Thickness 4 to 160 mm inclusive; width 500 mm and more
Scope, coils Thickness 4 to 25 mm
Dimensions and tolerances Remaining assortment requirements follow GOST 19903; state thickness accuracy and flatness on the order
Permitted inspection categories 3 only (Table 1). Categories 1, 2 and 4–7 are not listed. Category 3 specifies chemical-composition control, Table 2 tensile properties, a Table 5 180° bend, and a KCU impact test at +20 °C to Table 4
Chemical composition Shall conform to GOST 380 (clause 7.1.1.1). The only listed category specifies chemical-composition control. Clause 7.1.1.3 is not written for this grade. Numeric GOST 380 limits are not tabulated on this page
Tensile properties Table 2 for the listed category 3. Category 6 (Table 3) is not listed for this grade
Yield strength σT Table 2 minima, by thickness band, in the row shared by St4ps and St4sp. See Mechanical Properties
180° bend Table 5 row for St0, St4ps and St4sp: d = 2.5a / 3.5a / 3.5a. Not the St2/St3 1.5a row
Impact toughness Category 3 only: KCU at +20 °C to Table 4, in J/cm². Categories 4–7 are not listed
Delivery condition Clause 7.1.6, for the listed category 3 (in the categories 1–5 and 7 group): without heat treatment (hot-rolled), or thermomechanically treated, or heat-treated. Category 6 is not listed
Ultrasonic testing By agreement, to a class of GOST 22727; class and volume are not implied by the grade
Acceptance, marking and packaging GOST 7566, with the additions in the 2024 standard

GOST 14637 is a general-quality nonalloyed plate standard. It is not a boiler or pressure-vessel plate standard, and it is not a quality carbon structural plate standard. Do not copy figures from those systems onto a GOST 14637 order.

GOST 14637 St4sp Steel Plate Chemical Composition

Clause 7.1.1.1 of GOST 14637-2024 requires the chemical composition of the steel by ladle analysis of the ladle sample, and the permissible deviations in the finished product, to conform to GOST 380. This page does not tabulate GOST 380 heat-analysis limits. Confirm every chemistry cell against the applicable official GOST 380 table. This page is not a substitute for that table.

In Table 1, the only category listed for this grade (category 3) specifies chemical-composition control. Categories 1 and 2 are not listed, so a delivery without chemistry control is not a listed option. Ladle analysis and product deviations shall conform to GOST 380.

Clause 7.1.1.2 permits manufacture without a lower limit on carbon and manganese, except for plate intended for shipbuilding, wagon-building or welded cylinders, provided the mechanical properties of this standard are met. State that option on the order if it is required.

On purchaser request, clause 7.1.1.4 tightens sulphur and phosphorus for categories 1–5 to S not more than 0.040 % and P not more than 0.030 %. For this grade, the request applies when the listed category 3 is ordered. Categories 6 and 7, for which each of these elements shall not exceed 0.025 %, are not listed for this grade. If the tighter request limits are required, state them on the order.

Clause 7.1.1.3, which allows a stated reduction of a carbon or manganese lower limit at thickness up to 10 mm for Ст3кп, Ст3пс and Ст3сп, is not written for St4sp. Do not apply that option to this grade.

For subsequent hot-dip galvanizing, clause 7.1.1.5 allows agreed silicon classes. Classes B (silicon 0.14 % to 0.25 %) and D (silicon 0.25 % to 0.35 %) are the classes written for killed (sp) steel. Class A is written for rimmed (kp) steel and is not the class for this killed grade. Galvanizing class is an agreed option, not a default.

A maximum sign is an upper limit, not a target addition. Product-analysis deviations belonging to GOST 380 must not be used to widen ladle-analysis order limits. Numeric GOST 380 element ranges are not tabulated on this page.

GOST 14637 St4sp Steel Plate Mechanical Properties

Clause 7.1.7.1 requires the tensile properties of plate in categories 1–5 and 7 to meet Table 2. For this grade, only category 3 is listed; the Table 2 values below apply to that listed category. Units are N/mm² for strength (the unit used in the 2024 tables) and % for elongation δ5. Table 2 heading is “not less than or within limits.”

Property Thickness Requirement (Table 2)
Tensile strength σB, N/mm² All thicknesses in the 2024 scope 410–530
Yield strength σT, N/mm² ≤20 mm ≥265
Yield strength σT, N/mm² >20 mm to 40 mm inclusive ≥255
Yield strength σT, N/mm² >40 mm to 100 mm inclusive ≥245
Yield strength σT, N/mm² >100 mm ≥235
Elongation δ5, % ≤20 mm ≥24
Elongation δ5, % >20 mm to 40 mm inclusive ≥23
Elongation δ5, % >40 mm ≥21

This Table 2 row is shared by St4ps and St4sp (tensile strength 410–530 N/mm²). A shared row is not interchangeability: the two grades differ by deoxidation. GOST 14637 St5ps Steel Plate and GOST 14637 St5sp Steel Plate have a higher tensile-strength cell (490–630 N/mm²), and GOST 14637 St5Gps Steel Plate has a different cell (450–590 N/mm²). GOST 14637 St3sp Steel Plate has a lower cell (370–480 N/mm²). Do not take figures from those other rows, and do not take yield or tensile values from another product standard. The 1989 rimmed Ст4кп is not a 2024 grade and has no Table 2 row in this edition.

Table 2 footnotes that apply when the corresponding cell is a specified value include the following. For coil plate of thickness over 12 mm to 25 mm inclusive, the mechanical-property norms are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. The upper tensile-strength limit may be increased by not more than 50 N/mm² while the other mechanical-property norms are observed, and by agreement with the purchaser without limiting the upper bound. By agreement, for thickness over 20 mm, the yield value may be reduced by 10 N/mm². Table 2 also permits a stated reduction of elongation for thinner plate: for thickness up to 8 mm inclusive, by 1 % absolute for each millimetre of thickness reduction; for thickness over 8 mm, by 1 % absolute. Confirm the application of this footnote against the official table when thin plate is ordered.

By agreement between the manufacturer and the purchaser, plate of St4ps and St4sp may be supplied to Table 2 with a tensile-strength range of 410 to 590 N/mm² inclusive, in place of the grade’s own Table 2 tensile-strength cell (410–530 N/mm²). State that agreed range on the order if it is required.

Clause 7.1.8 requires the plate to withstand a 180° cold bend on a mandrel of the diameter in Table 5. At the bend there shall be no fracture, delamination or cracks.

Property Thickness (a = plate thickness) Requirement (Table 5)
180° cold bend, mandrel diameter d ≤20 mm d = 2.5a
180° cold bend, mandrel diameter d >20 mm to 40 mm inclusive d = 3.5a
180° cold bend, mandrel diameter d >40 mm d = 3.5a

These 2.5a / 3.5a / 3.5a diameters are the Table 5 row written for St0, St4ps and St4sp. They are not the tighter 1.5a / 2.5a / 2.5a diameters used for the St2 and St3 grades (except category 6), and they are not the 3.5a / 4.5a / 4.5a diameters used for St5ps, St5sp and St5Gps. Do not take mandrel diameters from another grade’s Table 5 row. Category 6, which has a further Table 5 row, is not listed for this grade.

Clause 7.1.7.3 requires impact tests of categories 3–7 to meet Table 4. For this grade, only category 3 is listed, so the applicable Table 4 cells are the category-3 KCU values at +20 °C (J/cm², not less than). Table 1 footnote 6, which requires category 3 of Ст3кп to be manufactured by agreement, does not name this grade. Table 1 footnote 4, which requires manufacture by agreement for categories 2 and 3 of St3ps and St3sp at thickness 5 mm and more (except tube plate), likewise does not name this grade. Do not treat those footnotes as conditions written for St4sp.

Thickness KCU at +20 °C, J/cm² (Table 4, category 3)
4.0 to 10.0 mm inclusive ≥78
>10.0 to 30.0 mm inclusive ≥69
>30.0 to 40.0 mm inclusive ≥49
>40.0 to 60.0 mm inclusive ≥49*
>60.0 mm Determined for statistical data (+)

Units are joules per square centimetre (J/cm²), not absorbed energy in joules. A plus sign means the value is determined for statistical data and is stated in the quality document; this page does not replace a plus with a number. Values marked with an asterisk are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. On one specimen, a 30 % reduction of the impact value is allowed provided the average of the test results is not below the Table 4 norm; the average is stated in the quality document. For coil plate of thickness over 12 mm to 25 mm inclusive, the impact norms are likewise optional for those two years. On purchaser request, impact work in joules may be determined instead of impact toughness, with limit values agreed between the manufacturer and the purchaser.

Categories 4–7 are not listed for this grade; those Table 4 columns are not tabulated here. Category 6 tensile properties (Table 3) are not applicable.

GOST 14637 St4sp Steel Plate Delivery Conditions

Under clause 7.1.6, plate of categories 1–5 and 7 is manufactured without heat treatment (in the hot-rolled condition), or in the thermomechanically treated condition, or in the heat-treated condition. Category 6 is manufactured in the thermomechanically treated or heat-treated condition only; category 6 is not listed for this grade. State the required delivery condition on the order. If the condition is omitted, do not assume a heat-treated or thermomechanically treated delivery from the grade name alone; for the listed categories, which all fall in the 1–5 and 7 group, the manufacturer may supply the plate hot-rolled. Record the actual condition on the quality document.

St4sp may be ordered in category 3 only. Categories 1, 2 and 4–7 are not listed for this grade in Table 1. State the category on the order. There is no listed chemistry-free, impact-free category-1 option, and there is no listed category-6 thermomechanically treated or heat-treated-only option. Category 3 includes the Table 4 KCU test at +20 °C. A usual hot-rolled delivery is not a substitute for an agreed thermomechanical or heat-treatment condition when the project requires one.

GOST 14637 St4sp Steel Plate Weldability

On purchaser request, clause 7.1.2 allows plate to be supplied with a weldability guarantee, designated in the standard as GS. That guarantee is ensured by limiting the ladle-analysis carbon content to not more than 0.22 %. If a weldability guarantee is required, state it on the order. The designation alone does not include it.

This page does not give preheat, interpass, heat-input or post-weld heat-treatment figures. The fabricator is responsible for welding-procedure qualification, consumable selection, preheat and any post-weld heat treatment required by the project specification. Do not take those figures from another standard or from a handbook and apply them as GOST 14637 rules.

St4sp is a killed (sp) steel in a higher carbon class than the St3 grades. Semi-killed and killed St4 plates, and the St5 grades, are not automatic welding substitutes for each other. Do not assume that a procedure qualified on GOST 14637 St4ps Steel Plate, on an St3 grade, or on an St5 grade is valid for this grade without qualification. Because official GOST 380 chemistry limits are not tabulated on this page, do not assume that ladle carbon is already at or below 0.22 %. If the weldability guarantee is required, order it and confirm the carbon restriction against the official texts.

GOST 14637 St4sp Steel Plate Tolerances

Remaining assortment requirements — dimensions, shape and permissible deviations beyond the thickness and width scope in clause 6.2.1 — follow GOST 19903. State the required thickness-accuracy class, edge condition and, for plate supplied as sheets, the flatness class on the order. This page does not tabulate numerical deviation limits from GOST 19903.

Surface quality is specified in clause 7.1.3 of the 2024 standard. Defects of the types listed there are not permitted. Dressing is allowed within the depth and area limits stated in that clause; confirm those limits against the official text. Delamination on ends and on untrimmed edges is not permitted.

Ultrasonic testing is not a default requirement. By agreement, clause 7.1.9 allows plate in sheets to be supplied with ultrasonic testing to a class of GOST 22727. The continuity class and the test volume are not implied by the grade or the category; state them on the order if they are required.

GOST 14637 St4sp Steel Plate Applications and service limits

GOST 14637-2024 is a general-quality nonalloyed plate specification. Typical uses are structural and general fabrication where the ordered category, thickness and delivery condition of this grade meet the project specification. This page does not assign a service temperature, a pressure rating or a code-allowed stress from the grade name. The purchaser and the designer remain responsible for fitness for the intended duty.

St4sp is listed only in category 3, so every listed supply includes chemical-composition control and a KCU impact test at +20 °C. That listing does not by itself qualify the plate for a designated service temperature: Table 4 states a test temperature and impact values in J/cm², not an allowable operating temperature. A killed (sp) deoxidation and a higher Table 2 tensile class than St3 do not qualify the plate for a pressure duty. This grade is not a boiler or pressure-vessel plate and is not a quality carbon structural plate; do not copy figures from those systems onto the order.

Compare St4sp with related GOST 14637 grades

The figures in the table below are from GOST 14637-2024 Table 2, Table 1 and Table 5. They compare grades inside this standard. A shared carbon class, a shared yield cell or a nearby tensile-strength range is not interchangeability.

Grade Table 2 tensile σB, N/mm² Yield σT, ≤20 mm Elongation δ5, ≤20 mm Table 1 categories Table 5 mandrel d
GOST 14637 St3sp Steel Plate 370–480 ≥245 ≥26 1–7 1.5a / 2.5a / 2.5a
GOST 14637 St4ps Steel Plate 410–530 ≥265 ≥24 3 only 2.5a / 3.5a / 3.5a
GOST 14637 St4sp Steel Plate (this page) 410–530 ≥265 ≥24 3 only 2.5a / 3.5a / 3.5a
GOST 14637 St5ps Steel Plate 490–630 ≥285 ≥20 1–2 3.5a / 4.5a / 4.5a
GOST 14637 St5sp Steel Plate 490–630 ≥285 ≥20 1–2 3.5a / 4.5a / 4.5a
GOST 14637 St5Gps Steel Plate 450–590 ≥285 ≥20 1–2 3.5a / 4.5a / 4.5a

St4ps and St4sp share a full Table 2 row (410–530 N/mm²) and the same Table 5 bend diameters (2.5a / 3.5a / 3.5a), and both are listed only in category 3. The difference is deoxidation. GOST 14637 St3sp Steel Plate has a lower tensile-strength cell and is listed in categories 1–7, with tighter Table 5 diameters. GOST 14637 St5ps Steel Plate and GOST 14637 St5sp Steel Plate have a higher tensile-strength cell (490–630 N/mm²), are listed only in categories 1 and 2 (no impact), and use larger Table 5 mandrels (3.5a / 4.5a / 4.5a). GOST 14637 St5Gps Steel Plate has a lower tensile-strength cell than those St5 plates (450–590 N/mm²) and the same St5 category listing. None of those relationships is interchangeability. The 1989 rimmed St4kp is not a 2024 grade.

Purchasers may compare the St4 class with GB/T 700 Q275A. A comparison is not an equivalent. That grade belongs to another product standard, with its own chemistry, tensile, impact and delivery rules. See also the GB/T 700 hub. Do not copy a yield, impact or chemistry figure from that page onto a GOST 14637 order.

GOST 14637 St4sp Steel Plate Equivalent Material Grade

The entry below is a related comparison, not an equivalent grade. GOST 14637-2024 does not publish a one-to-one equivalent-grade table for this designation. A comparable tensile class in another standard is not a substitute: chemistry, deoxidation, impact category and delivery condition must each be checked against the official texts.

Standard Country-Region Equivalent Grade Note
GB/T 700 China GB/T 700 Q275A Related comparison with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.

If a project specification names one of those other grades, order that specification. If it names St4sp under GOST 14637-2024, order this grade and the required category. Do not treat a cross-reference as a certified equivalent.

Why choose Us

SHH STEEL produces and exports GOST 14637 plate, including St4sp. We review the killed (sp) deoxidation, the Table 2 row shared by St4ps and St4sp (410–530 N/mm²), the agreed 410–590 N/mm² tensile option, the category-3 listing, and the Table 5 mandrels 2.5a / 3.5a / 3.5a before production, and we state the actual results on the quality document. We do not treat a shared Table 2 cell or a commonly compared foreign grade as a substitute for the ordered designation.

Orders are accepted against GOST 14637-2024. Enquiry details should include grade, category, thickness, width, length or coil mass, quantity, delivery condition and any agreed options (weldability guarantee, galvanizing class, tighter sulphur and phosphorus, ultrasonic class). See the GOST 14637 hub for the product family.

Our Service

Supply covers production to the ordered 2024 requirements, mill documentation, and export packing and shipment. Quality documents record the actual ladle analysis, tensile results and, where the category requires them, impact results, including any characteristic that Table 2 or Table 4 marks as determined for statistical data. Ultrasonic testing, a weldability guarantee and a galvanizing class are supplied when they are agreed on the order, not by default.

To enquire, state GOST 14637-2024, grade St4sp, the Table 1 category, dimensions, quantity and the required options. SHH STEEL will confirm manufacturability and the inspection plan against that order. This page is a product description; the official standard and the quality document govern acceptance.

FAQ

What is GOST 14637 St4sp steel plate?

St4sp (Ст4сп) is the killed (sp) St4 grade under GOST 14637-2024. In Table 2 it shares a mechanical row with GOST 14637 St4ps Steel Plate (tensile strength 410–530 N/mm²). A shared row is not interchangeability. It is listed in Table 1 category 3 only, which includes chemical-composition control and a KCU impact test at +20 °C. The 1989 rimmed St4kp is not a 2024 grade.

Which inspection categories apply to St4sp?

Table 1 lists St4sp in category 3 only. Categories 1, 2 and 4–7 are not listed. Category 3 specifies chemistry control, Table 2 tensile properties, a Table 5 180° bend (d = 2.5a / 3.5a / 3.5a), and KCU at +20 °C to Table 4. Category 6 is not a listed option. State the category on the order.

What are the Table 2 tensile properties of St4sp?

Tensile strength is 410–530 N/mm². Yield minima are 265, 255, 245 and 235 N/mm² in the four thickness bands. Elongation δ5 minima are 24, 23 and 21 %. By agreement, St4ps and St4sp may be supplied to Table 2 with a tensile-strength range of 410 to 590 N/mm² inclusive. Category 6 (Table 3) is not listed for this grade.

Is St4sp interchangeable with St4ps or with the St5 grades?

No. GOST 14637 St4ps Steel Plate shares this Table 2 row but is semi-killed. GOST 14637 St5ps Steel Plate and GOST 14637 St5sp Steel Plate have a higher tensile-strength cell (490–630 N/mm²), are listed only in categories 1 and 2 (no impact), and use different Table 5 mandrels (3.5a / 4.5a / 4.5a). GOST 14637 St5Gps Steel Plate has a lower cell (450–590 N/mm²) than those St5 plates. A shared row or a nearby tensile class is not interchangeability.

Where is the chemical composition of St4sp specified?

Clause 7.1.1.1 requires ladle analysis and product deviations to conform to GOST 380. This page does not tabulate those GOST 380 cells. Confirm them against the applicable official GOST 380 table. The only listed category already specifies chemistry control. Clause 7.1.1.3 is not written for this grade. Tighter sulphur and phosphorus follow clause 7.1.1.4 when requested for the listed category 3.

Enquire about GOST 14637 St4sp Steel Plate

Enquire for GOST 14637 St4sp Steel Plate to GOST 14637-2024. State the category (3 only; categories 1, 2 and 4–7 are not listed), thickness, width, length or coil mass, quantity, delivery condition and any agreed options. SHH STEEL will review the killed (sp) deoxidation, the Table 2 row (410–530 N/mm²), the Table 5 mandrels (2.5a / 3.5a / 3.5a) and the category-3 impact test before quoting production and export.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X